Qi He,
Xingyu Liu and
Xiang Wu
*
School of Materials Science and Engineering, Shenyang University of Technology, Shenyang 110870, P. R. China. E-mail: wuxiang05@163.com
First published on 9th August 2024
Recently, ternary metal oxides as cathode materials have been the focus of research into supercapacitors owing to their high power density and cost-efficient features. The development of excellent electrode materials is the key to improving supercapacitor total performance. Herein, we report several kinds of NiMoO4 nanostructures grown on nickel foam using a simple hydrothermal strategy. The assembled hybrid devices show an energy density of 35.9 W h kg−1 at a power density of 2708 W kg−1. After repeated charging and discharging cycling and bending tests, they show excellent durability performance and mechanical stability performance.
Compared to binary transition metal oxides, the ternary NiMoO4 compound shows richer oxidation states because of the synergistic effect of bimetallic interactions.18–20 It results in highly reversible redox reactions and excellent electrochemical performance.21,22 In previous reports, Wang et al. prepared Pr2CrMnO6 electrode materials with a specific capacitance of 177.4 F g−1 at 2 A g−1.23 Co2S4@NiMo-LDH nanocomposites deliver a specific capacitance of 1346 F g−1 at 1 A g−1 and after 10
000 cycles, the capacitance retention rate is 80%.24 He's group synthesized a NiMoO4–Ag/rGO product with 1132.8 F g−1 at 1 A g−1, which retains 95% of the initial capacitance after 1000 cycles.25 We also prepared NiMoCo-LDH materials on nickel foam using a hydrothermal route. It showed a specific capacitance of 1284.2 F g−1 at 1 A g−1 and a capacitance retention of 85.3% after 8000 cycles.26 Although much progress has been made in the past two decades, this has been made using excessively complex preparation routines to obtain similar specific capacities. We have reduced the complexity of the manufacturing process and production cost via a simple preparation method to increase the practical value of supercapacitors. NiMoO4 nanorods on NF for supercapacitors possess the advantages of low cost, excellent electrical conductivity, excellent chemical stability, light weight, flexibility and high porosity. The open space between the nanorods allows easy diffusion of electrolytes and avoids the use of polymer binders.27
In this work, we synthesize several NiMoO4 samples on nickel foam (NF) using a simple hydrothermal process. Many characterization studies are performed to assess the microstructural and capacitance performance of the as-obtained samples. By adjusting the Ni/Mo molar ratio, it is found that the NiMoO4-2 electrode material delivers a specific capacitance of 1194 F g−1 of 1 A g−1 when Ni/Mo = 1
:
1. Moreover, the as-prepared samples are used as cathodes in the assembly of asymmetric supercapacitors (ASC). They provide an energy density of 35.9 W h kg−1 at a power density of 2708 W kg−1. At the same time, the as-fabricated devices retain 89.2% of initial capacitance after 10
000 cycles. Also, the bending experiments demonstrate their outstanding mechanical stability, indicating potential for applications in flexible electronics fields.
| Labels | Ni(NO3)2·6H2O | Na2MoO4·2H2O | Urea | NH4F | Molar ratios |
|---|---|---|---|---|---|
| Ni(OH)2 | 2 | 0 | 1 | 1 | 2 : 0 |
| NiMoO4-1 | 4 | 2 | 1 | 1 | 2 : 1 |
| NiMoO4-2 | 2 | 2 | 1 | 1 | 1 : 1 |
| NiMoO4-3 | 2 | 4 | 1 | 1 | 1 : 2 |
:
2
:
1 in an onyx mortar and ground by adding anhydrous ethanol. Each time, the ethanol in the agate mortar was completely ground and evaporated before the next grinding. After the third time, NMP solution was added dropwise to the agate mortar and ground well. The resulting slurry was uniformly coated on the pre-treated NF with a spatula and dried in a vacuum oven at 60 °C for 10 h.
| C = IΔt/m | (1) |
| Q = It = CmΔV | (2) |
| m+/m− = Cm−(ΔV)−/Cm+(ΔV)+ | (3) |
The energy density (E) and power density (P) of the NiMoO4-2 samples were calculated as follows:
| P = 1800CΔV2/Δt | (4) |
![]() | ||
| Fig. 1 Structural characterization. (a) XRD patterns. (b)–(d) XPS spectra of the NiMoO4-2 sample. (e) and (f) N2 adsorption–desorption isotherms (the insets: the pore size distribution curves). | ||
XPS is then employed to exam the surface chemical composition of NiMoO4-2 electrode. From the Ni 2p spectra in Fig. 1b, two spin–orbit peaks at 856.1 and 873.8 eV correspond to Ni 2p3/2 and Ni 2p1/2, respectively. The peaks at 879.58 and 861.88 eV can be assigned to the satellites.29 The photoelectron spectra of Mo 3d (Fig. 1c) show the characteristic peaks of Mo 3d3/2 at 232.2 eV and Mo 3d5/2 at 235.4 eV. It proves that Mo6+ possesses a high oxidation state.30 Fig. 1d is divided into three peaks: O1 (530.1 eV), O2 (531.3 eV) and O3 (532.9 eV) peaks. They represent metal–oxygen bonds (M–O), –OH bonds and oxygen species in the adsorbed water/defect, respectively.31 Fig. 1e and f show the N2 isotherms of the two samples with a typical IV isotherm loop. It demonstrates that the samples possess a mesoporous structure and a broad pore-size distribution. The NiMoO4-2 products possess a larger specific area (48.589 m2 g−1) than Ni(OH)2 samples (18.054 m2 g−1). In addition, the total pore volumes of the NiMoO4-2 and Ni(OH)2 samples are 0.175 and 0.056 cm3 g−1, respectively. The results reveal that the introduction of Mo elements increase the specific surface area and active sites.
After that, we study the morphologies and structures of the samples. As shown in Fig. 2a and e, the Ni(OH)2 microplates overlap with each other. They present an average thickness of 100 nm. With the addition of Mo, the crystal structure and growth rate of the NiMoO4 material change compared to the Ni(OH)2 sample, resulting in a change in the morphology. From Fig. 2b and f, when the ratio of Ni/Mo is 2
:
1, the NiMoO4-1 sample evolves into a rod-like nanostructure with a high specific surface area relative to the nanoplate. When the Ni/Mo molar ratio decreased to 1
:
1 (Fig. 2c and g), the nanorod density increased. It provides more transmission channels for ion diffusion and storage.32 At this time, the nanorods have a diameter of 100 nm. As shown in Fig. 2d and h, the nanorods begin to aggregate and adhere when the ratio of Ni/Mo is further reduced to 1
:
2, which blocks the electron charge channels. A low magnification TEM image (Fig. 2i) shows that NiMoO4-2 sample has a diameter of 100 nm, which is consistent with the above SEM results. The corresponding HRTEM (Fig. 2j) reveals that the calculated d-spacing of 0.427 nm is well matched with the NiMoO4-2 crystal phase (JCPDS No. 13-0128). From Fig. 2k, the element mappings demonstrate that Ni, Mo and O elements are uniformly distributed on the surface of the nanorod.
Then we examine the electrochemical performance of all the samples in a three-electrode system. Fig. 3a presents the CV curves of the several electrode materials. The curve area of as-prepared NiMoO4-2 product is larger than that of other products. The reaction dynamics during the electrochemical process can be described as follows:33
| NiMoO4 ↔ Ni2+ + MoO42− | (5) |
| Ni2+ + 2OH− ↔ Ni(OH)2 | (6) |
| Ni(OH)2 + OH− ↔ NiOOH + H2O + e− | (7) |
Although Mo is not involved in the electrochemical process, it can improve the conductivity of the hybrid electrode. The GCD curve of four samples at 1 A g−1 are presented in Fig. 3b. It can be found that the specific capacity of the NiMoO4 material shows a growing and subsequently declining pattern as the addition ratio of Mo element increases. The reason for this is that the nanorod consistency increases with the increase of Mo ratio in the early stage, which in turn makes the material obtain more effective active sites and the electrochemical performance is enhanced. At Ni/Mo = 1
:
1, the nanorod density reaches the optimum and the specific capacity reaches the maximum. With the further increase of the addition ratio of Mo element, the density of the nanorod structure of NiMoO4 material increases again and adhesion occurs, which affects the adequate contact between the electrolyte and the active material as well as the smoothness of the electron charge inlet and outlet channels. Thus, the effective active area of the electrode material was reduced, leading to a decrease in the specific capacitance. Fig. 3c indicates their CV curves at various scan rates. Furthermore, the peak currents (anodic and cathodic) present a slight increase as the scan rate increases. It could be attributed to the reaction kinetics of the electrode materials. As shown on the NiMoO4-2 electrode GCD curves (Fig. 3d), there are obvious charging and discharging platforms at different current densities, indicating their battery-type characteristics. At the current density of 1, 2, 4, 6, 8 and 10 A g−1, the specific capacitance of the electrode materials is 1194, 984, 824, 612, 512 and 420 F g−1, respectively. Electrochemical impedance spectroscopy (EIS) of the devices are shown in Fig. 3e. For a high-frequency region, NiMoO4-2 electrode possesses an internal resistance (Rs) value of 0.53 Ω, which is superior to Ni(OH)2 (0.81 Ω), NiMoO4-1 (0.65 Ω) and NiMoO4-3 (0.55 Ω) electrode materials. The larger the linear slope of the low frequency region, the smaller the diffusion impedance (Zw). The inset shows the EIS of the device before and after the cycling. Fig. 3f indicates the specific capacitance of the samples at 1, 2, 4, 6, 8 and 10 A g−1. NiMoO4-2 electrode delivers three times larger specific capacitance than NiMoO4-1 and NiMoO4-3 electrodes at a current density of 1 A g−1. It also maintains a moderate specific capacitance at high current densities. Fig. 3g depicts the slope values of anode and cathode peaks. The b values of NiMoO4-2 nanorod are 0.508 and 0.599, respectively. This implies that surface capacitance and diffusion control both contribute to the current response of the NiMoO4-2 electrode. Fig. 3h shows the surface capacitive contribution and diffusion controlled one of NiMoO4-2 at different scan rates. The diffusion controlled capacity reduces with the scan rate increasing. This is due to the limited diffusion time. The surface capacitive contributions reach 78.4% at 100 mV s−1, which indicates fast reaction kinetics. Fig. 3i presents the cycling curves of four electrode materials at the current density of 10 A g−1. It is found that NiMoO4-2 electrode material keeps a retention rate of 84% after 10
000 cycles, which is better than other electrode materials. NiMoO4-2 electrode material during 1500 times, it is completely saturated by the electrolyte, thus increasing the specific capacity of the material. However, as the number of cycles increased, the internal microstructure of the electrode material collapsed, thus decreasing the specific capacity.
Also, we fabricate ASC with a sandwich structure to explore the practical applications. Fig. 4a indicates the CV curves of active carbon and NiMoO4-2//AC samples at 100 mV s−1. The device reaches a theoretical potential of 1.6 V. From Fig. 4b, the CV curves of the device retain similar shapes and prove to have good reversibility as scan rates increase. The corresponding GCD curves (Fig. 4c) reveal that the device presents a specific capacitance of 115 F g−1 at a current density of 1 A g−1. Fig. 4d indicates the EIS of the device with a Rs value of 1.28 Ω, which proves its excellent electrical conductivity and the inset above left shows the appropriate equivalent circuit. The lower right inset shows the increase in the Rs value to 1.99 after cycling, indicating the decay of the capacitance. As shown in Fig. 4e, the device achieves the energy density of 36.03 W h kg−1 when the power density is 2699 W kg−1, and it can retain 25.5 W h kg−1 at 16
200 W kg−1. Table 2 lists the power and energy densities of several reported devices.34–37 It demonstrates that our assembled device is dominant compared with the others. Fig. 4f shows the capacitance contribution of NiMoO4-2//AC at different scan rates. The role of diffusion control is gradually substituted by surface-controlled behavior. The dominance of surface-controlled capacitance can be attributed to the limited ion diffusion time at high scan rates.
Finally, we explore the mechanical stability of the device. Fig. 4h shows the digital photos of the device bending at different angles. It is observed that the shapes of the CV curves maintain similar shapes with essentially the same area of integration when the device is twisted to 150°, 120°, 90° and 60°, respectively (Fig. 4g). From the cycling curves shown in Fig. 4i, the device retains 89.2% of its original capacitance at a current density of 1 A g−1 after 10
000 cycles. A blue LED lamp may be lit by three ASC devices connected in series for almost 9 min, demonstrating their potential applications in future energy storage fields.
:
1. The electrode materials show improved specific capacity and stability during cycles due to the synergistic effect of high conductivity Ni and Mo ions. In addition, the assembled ASC delivers high energy and power density and shows excellent mechanical stability. The reported synthetic protocol can be widened to prepare certain additional transition metals, such as sulfide and phosphide, for high-performance electrode materials for flexible capacitors.