Yang Baia,
Jianing He*ab,
Jinsheng Sunac,
Ren Wangc and
Ruifang Wanga
aState Key Laboratory of Oil and Gas Reservoir Geology and Exploitation, School of Oil & Natural Gas Engineering, Southwest Petroleum University, Chengdu, 610500, China. E-mail: w18351551338@126.com
bCollege of Petroleum Engineering, Liaoning Petrochemical University, Fushun, 113001, China
cKey Laboratory of Unconventional Oil & Gas Development (China University of Petroleum (East China)), Ministry of Education, Qingdao, 266580, China
First published on 4th July 2024
To treat the issue of increased resource wastage due to the higher plugging tendencies of oil-based drilling fluids (OBDF) relative to water-based drilling fluids, this study synthesized a ternary composite oil-absorbing resin and optimized its synthesis parameters. The influence of temperature variations on the resin's oil absorption capacity was assessed. Techniques such as infrared spectroscopy, scanning electron microscopy, TGA-DSC measurements, crosslinking degree analysis, contact angle analysis, X-ray photoelectron spectrometry analysis and examination of the resin's plugging mechanism were employed to investigate its molecular structure, oil absorption properties, and plugging efficiency. Additionally, the impact of various synthesis conditions on the oil absorption expansion rate of the oil-absorbing resin was examined. The findings indicate that the resin developed in this research maintains robust oil absorption capabilities at 160 °C, exhibiting an oil absorption expansion rate of 12.5 g g−1. At this temperature, the composite resin particles effectively sealed leaks of widths 0.25, 0.5, and 0.75 μm. Comparative analysis revealed that adding 3% of these resin particles to OBDF significantly enhanced the sealing of fractures. Remarkably, at 160 °C, OBDF amended with resin particles managed to completely seal fractures measuring 0.25 μm. The novelty of this study is attributed to the utilization of styrene for enhancing the resin's rigidity, coupled with the application of octadecyl methacrylate, which contains long-chain alkyl groups, to optimize the oil absorption and expansion characteristics of the oil-absorbing resin.
Currently, the majority of drilling fluids used in oil and gas field drilling engineering are categorized into water-based drilling fluid (WBDF),9–11 OBDF12–15 and synthetic-based drilling fluid.16,17 Among these, OBDF is often the preferred option for ultra-deep and complex wells due to its high-temperature resistance, superior lubrication, and enhanced wellbore stability. However, as OBDF systems continue to evolve, the issue of well leakage has become increasingly evident. On the one hand, the predominantly hydrophilic nature of the original rock surfaces within formations and the use of wetting agents in OBDF transform these surfaces from hydrophilic to oleophilic. Conversely, the requirement for oil-based drilling fluid plugging materials to exhibit excellent dispersibility in the oil phase necessitates that these materials possess an abundance of lipophilic functional groups. Consequently, this characteristic prevents the plugging material from forming non-covalent interactions, such as ionic and hydrogen bonds, with the oleophilic rock wall. During drilling, capillary forces can cause the wellbore wall rocks to adsorb both water and oil phases, enlarging the gap between fractured rock layers and thus heightening the risk of well leakage. Additionally, the effective lubrication provided by OBDF facilitates its entry into fractures, potentially inducing hydraulic fracturing and consequent well leakage.18 Consequently, the exploration of OBDF-compatible plugging materials has emerged as a prominent research topic. Currently, over a hundred types of plugging materials are utilized at major drilling sites, yet the vast majority are designed for WBDF, with only a limited number being compatible with OBDF.19,20 As a result, in the event of well leakage, technicians often resort to WBDF-appropriate plugging materials, which tend to yield suboptimal sealing outcomes. In summary, identifying a plugging material that exhibits strong compatibility with OBDF represents a significant area of interest within the field.
Currently, the plugging materials deemed compatible with OBDF predominantly encompass oleophilic resins, oil-absorbing and expanding substances, oil-based cross-linked gels, and hydrophobic materials.21–23 Among these, resin-based materials have attracted extensive research interest owing to their excellent compatibility with OBDF. For instance, Li et al.14 developed butadiene styrene/nano-SiO2 (SBR/SiO2) composites through a continuous emulsion polymerization process. Their findings revealed that the integration of silica and styrene not only imparts significant pressure resistance to the composites but also enables SBR/SiO2 to penetrate shale formations where leakage occurs, substantially mitigating fluid intrusion. Additionally, Du30 synthesized nanometer polystyrene dodecyl acrylate (PSL) oil absorption resin using styrene (St) and lauryl acrylate (LMA) via a soap-free emulsion polymerization method. This process yielded a product with remarkable dispersion stability and oil absorption expansion capabilities, primarily attributed to the flexible macromolecular chains of dodecyl acrylate, which undergo expansion upon oil absorption, facilitating deformation and expansion. Nonetheless, despite these advances, the application of the aforementioned resin-based plugging agents in OBDF systems on-site is limited by high production costs and a lack of universality, hindering optimal compatibility. However, the above research results used as plugging agents, didn't discuss the contradiction between the dispersibility of plugging agents and their staying capacity in the loss channel. In this study, the plugging agent prepared by us can be dispersed in oil-based drilling fluids due to its lipophilicity. Additionally, it can also be seen that the plugging agent has certain staying capacity in the plugging experiment. Therefore, the resin prepared in this study is of great significance for the plugging problems encountered during oilfield development.
In this paper, the study has developed a novel high-temperature-resistant suspension polymerization resin (MMA-SMA-St) tailored for OBDF applications. The resin is synthesized using methyl methacrylate (MMA), stearyl methacrylate (SMA), and styrene (St) as monomers. Incorporating methyl methacrylate and styrene addresses the issue of flexible crosslinking instability, which is attributed to the lengthy carbon chain present in stearyl methacrylate. Furthermore, the employment of suspension polymerization offers a practical framework for the field application of this plugging material.
(1) |
The oil absorbency is calculated using the formula wherein G1 and G2 represent the weights of the resin before and after oil absorption, respectively. Unless otherwise specified, “oil absorbency” refers to the total oil absorbency.24
Reagent | Dosage | Reagent action |
---|---|---|
3# white oil | 240 g | Base oil |
Fatty acid polyamide | 9 g | Emulsifier |
Organic soil | 9 g | Leaf cutting agent, tackifier |
CaO | 9 g | Alkalinity regulator |
25% CaCl2 | 60 mL | Adjusting the oil–water ratio |
Barite (4.2 g cm−3) | 211 g | Weighting agent |
The rheological parameters of OBDF, such as the apparent viscosity (AV), plastic viscosity (PV), and yield point (YP) of OBDF, were determined through measurements of the viscosities at two shear rates of 600 rpm and 300 rpm at room temperature by using a ZNN-D6L rotational viscometer (Qingdao, China). Calculated from the values of Ø600 and Ø300 by the following formulas:14
Apparemt viscosity (AV) = 0.5Ø600 (mPa s) | (2) |
Plastic viscosity (PV) = Ø600 − Ø300 (mPa s) | (3) |
Yield point (YP) = 0.511(2Ø300 − Ø600) (Pa) | (4) |
The presence of multiple side chain groups significantly influences the oil absorption capacity of resins. This phenomenon is attributed to compounds with multi-side chain structures expanding the internal volume of the resin via crosslinking agents. Consequently, when oil molecules penetrate the resin, the interaction surface between the resin and oil molecules enlarges, leading to an increased resin expansion rate. Thus, the proportions of MMA and SMA monomers utilized in the synthesis critically affect the resin's oil absorption expansion rate. Fig. 2(a) demonstrates that as the MMA:SMA molar ratio escalates, the oil-absorbing capability of the resin progressively improves. It is observed that an augmentation in MMA correlates with a heightened oil absorption rate. Furthermore, the oil absorption rate peaks when the MMA:SMA molar ratio reaches 2:1.18 Below a 2:1 MMA:SMA molar ratio, the presence of SMA yields numerous cross-linking points within the resin. However, an excess of these points restricts the flexibility of chain segments in the resin, diminishing the oil absorption expansion rate. Conversely, when the ratio exceeds 2:1, a reduced SMA concentration leads to a scarcity of long alkyl side chains in the polymer, thereby decreasing oil absorption capability. Fig. 2(b) illustrates the impact of varying monomer ratios on the resin's oil absorption capacity, revealing an initial increase followed by a decrease in oil absorption with the rise in PVA concentration, peaking at a 2.5% PVA concentration. At low PVA concentrations, oil-soluble monomers experience inadequate dispersion in water, leading to monomer aggregation, increased impurities within the polymer, and a reduced oil absorption expansion rate. Conversely, excessively high concentrations of PVA result in over-dispersion of monomers, which adversely affects the conditions conducive to polymerization, thereby diminishing the oil absorption rate.
Fig. 2(c) depicts the curve correlating the content of cross-linker N,N′-methylenebisacrylamide with the resin's oil absorption capacity. At lower MBA concentrations, the polymer exhibits fewer cross-linking points, resulting in a less effective cross-linking network within the resin. This insufficiency was observed during experiments where a minimal cross-linking agent concentration resulted in a product that was turbid and challenging to purify. As illustrated in Fig. 2(c), a progressive increase in MBA concentration led to the formation of a densely cross-linked structure within the resin. This structure facilitates oil molecule ingress via capillary action, with increasing numbers of oil molecules causing cross-linking points to rupture, allowing the long alkyl side chains within the resin to extend and the resin to absorb oil and swell. Furthermore, a higher degree of cross-linking enhances the resin's oil storage capacity, thereby augmenting its expansion rate, as indicated by Zhang's research.32 The optimal oil absorption rate was observed at the MBA concentration of 1.5%; beyond this point, the oil absorption rate declined. This decrease is attributed to higher cross-linking agent concentrations resulting in shorter chain segments between cross-linking points, reducing their mobility and, consequently, the resin's swelling capability.
Fig. 2(d) illustrates the influence of benzoyl peroxide (BPO) on the oil absorption characteristics of the resin, with the oil absorption expansion ratio peaking at a BPO concentration of 1.25%. Given the employment of oil-soluble monomers in the synthesis process, the oil-soluble free radical initiator BPO is utilized accordingly. BPO is recognized as an effective initiator for the synthesis of acrylic ester polymers.33 When the amount of BPO was low, the internal crosslinking degree of the resin was small, the contact area between oil molecules and polymers was also small, and the oil absorption rate decreased. The effect of initiators on the crosslinking degree of polymers had a peak. When there were too many initiators, not only would they not increase the oil absorption rate of the resin, but they would also affect the formation of polymer crosslinking structure and reduce the oil absorption rate of the resin.
Fig. 3 The results of contact angle: (a) the contact angle of white oil on the resin film surface under air conditions; (b) the contact angle of water on the resin film surface under air conditions. |
The resin structure was investigated using XPS, and the results are shown in Fig. 4. As shown in Fig. 4(a), the resin contains three elements: C, N, and O, and the characteristic peak intensity of C element is the highest, while N element is the lowest. Fig. 4(b) shows the high-resolution XPS spectrum of C 1s of the resin. After deconvolution, four peaks can be found in the resin, the peaks with binding energy of 288.9 and 286.9 eV are CO and C–O, indicating that the resin contains SMA and MMA. The peak with a binding energy of 285.9 eV is C6H5−, indicating the presence of St. In addition, the peak representing CC was not found in the C 1s spectrum, indicating that the product does not contain reactive monomers. Fig. 4(c) shows the high-resolution XPS spectrum of N 1s of the resin. There were two peaks found in the resin. The peaks with binding energy of 402.13 and 399.78 eV are N–(CO)– and C–N–C, representing the presence of MBA. Fig. 4(d) shows the high-resolution XPS spectrum of O 1s of the resin. After deconvolution, three peaks can be observed in the resin, representing C–O–C, O–(CO)–C and OC–N. C–O–C, O–(CO)–C indicate the presence of SMA and MMA in the resin. The presence of OC–N indicates the containment of crosslinking agent MBA in the resin.
Fig. 5(a) displays scanning electron microscope (SEM) images of the resin at 1000× magnification, revealing an irregular surface adorned with numerous gully-like structures. This uneven topology augments the contact surface between the resin and oil molecules, significantly enhancing the oil absorption expansion rate. Fig. 5(b) provides an SEM image of the resin at 10000× magnification, showcasing the presence of round microporous structures on the surface. These micropores facilitate the penetration of oil molecules into the resin's interior, further extending the contact surface between them, thereby augmenting the oil absorption expansion rate.
Fig. 5 SEM picture of the resin: (a) SEM pictures of the resin magnified 1000 times; (b) SEM pictures of the resin magnified 10000 times. |
The polymer's molecular structure was examined using thermogravimetric analysis (TGA) coupled with differential scanning calorimetry (DSC). As depicted in Fig. 6(a), the resin's weight reduction occurs in three distinct phases. The initial phase of weight loss extends from room temperature to 356 °C, during which the TGA curve maintains a nearly constant slope. The weight loss rate up to 356 °C is minimal, at only 1.5%, attributed to the volatilization of solvents in the resin. In the subsequent phase, spanning 356–401 °C, the resin's weight decreases significantly, with the DTG (differential thermogravimetric) curve peaking at 380 °C, marking the onset of thermal degradation of the resins. At 401 °C, the residue is a mere 0.16%, indicating a high resin purity. Beyond 414 °C in the final phase, the resin transitions to carbon, and the TGA curve stabilizes, demonstrating the resin's commendable thermal stability. These results align closely with the TGA findings for nano-sized poly(styrene-lauryl acrylate),34 showcasing even greater purity. In addition, the glass transition temperature (Tg) was characterized by DSC shown in Fig. 6(b). According to the curve, the softening point of resin is 115 °C. The glass transition temperature (Tg) refers to the temperature corresponding to the transition from a glassy state to a highly elastic state. Most of the cracks that cause leakage are located in deep formations, where the temperature is generally above 100 °C. Therefore, when the resin enters the formation exceeds the Tg, the resin will transform into a high elastic state and enter the cracks due to the positive pressure difference. After oil absorption, the resin will expand to seal the leakage cracks.
The infrared (IR) spectroscopy results of the oil-absorbing resin are depicted in Fig. 7. Absorption peaks at 2923 and 2852 cm−1 correspond to the asymmetric and symmetric stretching vibrations of C–H in the methyl and methylene groups, respectively, alongside –CH.18 The peak at 1726 cm−1 is associated with the stretching vibration of the acrylate ester carbonyl (CO), denoting the incorporation of MMA chain segments within the resin. Peaks at 1447 and 1383 cm−1 are ascribed to the CC stretching vibrations in the benzene ring. Additionally, peaks at 806, 757, and 700 cm−1 are linked to the out-of-plane bending vibrations of hydrogen in the benzene ring, characteristic of monosubstituted benzene.34 The presence of styrene-acrylonitrile (SMA) chain segments is evidenced by peaks at 1187 and 1138 cm−1, representing the C–O bond stretching vibrations, and a peak at 989 cm−1, associated with the in-plane rocking vibration of –CH in the long-chain methylene group. Collectively, the IR spectroscopy results confirm the involvement of MMA, SMA, and styrene (St) in constructing the resin's skeletal structure. Furthermore, the absence of CC absorption peaks in the range of 1640–1675 cm−1 suggests a comprehensive synthesis reaction, where the unsaturated groups of the three monomers have engaged in grafting, leading to the formation of a three-dimensional network structure.
The results of the model rubber crosslinking density test are shown in Table 2. According to the result, the relaxation time of crosslinked signals is very short, while the relaxation time of the signals from the uncrosslinked portion is very long. The relaxation time represents the degree of freedom of hydrogen protons in the resin, indicating a high degree of resin cross-linking. In addition, the cross-linking density was 76.03 × 10−4 mol mL−1, indicating the formation of an internal cross-linking network structure in the resin. To a certain extent, the higher the cross-linking density of the resin, the more cross-linking bonds there are per unit volume of the resin, and the greater the degree of cross-linking. When oil molecules enter the interior of the resin, the cross-linking network is stretched by the oil molecules, causing the resin volume to increase and the oil absorption rate to increase.
T2A (ms) | T2B (ms) | Crosslinking density (10−4 mol mL−1) |
---|---|---|
0.13 | 1.27 | 76.13 |
Table 3 presents the outcomes of the electrical stability and rheological tests. These tests evaluated the rheological properties and demulsification voltage of drilling fluids before and after the incorporation of 3% resin, under various temperatures and aging conditions. Relative to drilling fluids devoid of resin, the apparent viscosity (AV), plastic viscosity (PV), and yield point (YP) exhibited increases both before and after aging. This rise is attributed to the addition of solid resin particles, which heightens the flow friction resistance among solids and liquids, as well as between the solids and liquids themselves. Furthermore, the introduction of resin particles markedly elevates the demulsification voltage, a consequence of the enhanced viscosity of the drilling fluid imparted by the resin particles, leading to a more stable emulsion and, hence, an increased demulsification voltage. Additionally, as illustrated in Table 3, the aging temperature's elevation significantly affects the rheological properties and demulsification voltage of the drilling fluid mud, suggesting commendable compatibility between the resin and mud.
Type | Aging temperature (°C) | Condition | AV (mPa s) | PV (mPa s) | YP (Pa) | Es (V) |
---|---|---|---|---|---|---|
Original OBDF | 120 | Before aging | 64 | 62 | 2 | 550 |
After aging | 66 | 63 | 3 | 541 | ||
Original OBDF | 140 | Before aging | 62 | 58 | 4 | 544 |
After aging | 65 | 61 | 4 | 542 | ||
Original OBDF | 160 | Before aging | 60 | 57 | 3 | 540 |
After aging | 58 | 54 | 4 | 533 | ||
With 3% resin | 120 | Before aging | 89 | 80 | 9 | 1290 |
After aging | 87 | 81 | 6 | 1287 | ||
With 3% resin | 140 | Before aging | 87 | 81 | 6 | 1256 |
0 | After aging | 88 | 83 | 5 | 1198 | |
With 3% resin | 160 | Before aging | 84 | 80 | 4 | 1100 |
After aging | 86 | 82 | 4 | 1088 |
Fig. 9 displays the experimental data on the oil absorption expansion rate of the resin at room temperature, as well as at 80, 120, 140, and 160 °C. Notably, at 160 °C, the resin's oil absorption expansion ratio reached 12.2. Research of the resin's oil absorption process at room temperature revealed that the resin's maximum oil absorption rate is governed by thermodynamics. Additionally, the resin's oil absorption saturation rate is primarily influenced by its crosslinking density and the solvation interactions between oil molecules and the resin's oleophilic groups. Consequently, with rising temperatures, the initial stage of oil absorption, dominated by molecular diffusion, facilitates greater contact between oil molecules and the resin surface, thereby increasing the number of oil molecules penetrating the resin's interior. In the subsequent stage, dominated by thermodynamic control, the interaction between oil molecules and the resin's oleophilic groups becomes more comprehensive, enhancing the solvation effect and thus the resin's expansion volume.
Type | Slit width (μm) | Condition | FLHTHP (mL) |
---|---|---|---|
Original OBDF | 0.25 | Before aging | 5 |
After aging | 7 | ||
Original OBDF | 0.5 | Before aging | 10 |
After aging | 10 | ||
Original OBDF | 0.75 | Before aging | Full loss |
After aging | Full loss | ||
With 3% resin | 0.25 | Before aging | 0 |
After aging | 0 | ||
With 3% resin | 0.5 | Before aging | 0 |
After aging | 1 | ||
With 3% resin | 0.75 | Before aging | 2 |
After aging | 2.6 |
Fig. 10 illustrates the state of the crack plate during the plugging experiment with a crack width of 0.25 μm. The regions highlighted in red represent resin particles. Observation reveals that resin particles accumulate within the crack. Subject to high temperature and pressure conditions, these particles undergo deformation and penetrate the crack under compressive forces. Owing to the resin's expansion and viscosity within the environment of oil molecules, it remains lodged within the crack, thereby effectively sealing the leak.
Component | Testing conditions | Invasion depth (cm) | Lost circulation (cm) |
---|---|---|---|
2% resin | 30 min, 0.7 MPa | 3.8 | Zero |
4% resin | 30 min, 0.7 MPa | 1.3 | Zero |
6% resin | 30 min, 0.7 MPa | 0.6 | Zero |
Traditional plugging materials often necessitate specific particle sizes to effectively seal lost circulation zones. In scenarios involving smaller void spaces, these rigid plugging materials must be crushed and resized before incorporation into the plugging mud. Conversely, the resin-based plugging materials developed in this study are capable of adapting to various pore sizes in loss channels, thanks to their inherent variability. Furthermore, the incorporation of styrene (St), with its benzene ring structure, imparts a degree of pressure resistance to the mixture. Beyond this, the resin particles exhibit a certain viscosity upon oil absorption, allowing them to persist within the leakage channels. This capacity enables them to form a pressure-sealing layer possessing adequate strength to mitigate fluid loss effectively.
Fig. 11 The schematic diagram of resin entering the leakage channel to block the leak after a well leakage occurs underground. |
(2) The molecular structure and characteristics of the resin were investigated using SEM, TG, and IR, providing insights into the resin's synthesis and oil absorption mechanism. This analysis further substantiated the process by which oil molecules infiltrate the resin, resulting in its expansion.
(3) This study examines the impact of variations in MMA: SMA, MBA, PVA, and BPO ratios on the oil absorption capabilities of oil-absorbing resins to identify the composition that yields the highest oil absorption performance.
(4) The composite resin particles were utilized to plug fractures with widths ranging from 0.25 to 0.75 μm, demonstrating a filtration loss of 2.6 mL under high temperature and high pressure conditions in 0.75 μm cracks. Furthermore, the sealing mechanisms of the resin particles within geological formations were elucidated.
(5) The results of this study can be used in the field of drilling fluid plugging. The resin mentioned in this article can seal cracks of different widths, which can effectively solve the problem of difficult plugging in drilling operations.
This journal is © The Royal Society of Chemistry 2024 |