aDoctoral School of the Rzeszów University of Technology, Rzeszów University of Technology, Powstańców Warszawy 12, 35-959 Rzeszów, Poland
bDepartment of Photomedicine and Physical Chemistry, Medical College of University of Rzeszów, University of Rzeszów, Warzywna 1A Street, 35-310 Rzeszów, Poland
cInstitute of Chemistry, University of Silesia in Katowice, Szkolna 9, 40-006 Katowice, Poland
dDepartment of Organic Chemistry, Bioorganic Chemistry and Biotechnology, Silesian University of Technology, Krzywoustego 4, 44-100 Gliwice, Poland. E-mail: Slawomir.Boncel@polsl.pl
eCentre for Organic and Nanohybrid Electronics (CONE), Silesian University of Technology, Konarskiego 22B, 44-100 Gliwice, Poland
fDepartment of Physical Chemistry and Technology of Polymers, Silesian University of Technology, ks. Marcina Strzody 9, 44-100 Gliwice, Poland
gDepartment of Physics and Medical Engineering, Rzeszów University of Technology, Powstańców Warszawy 6, 35-959 Rzeszów, Poland. E-mail: gzyla@prz.edu.pl
First published on 27th August 2024
In the field of radiological protection, there is a growing interest in nano- and microcomposites due to their unique physicochemical properties, flexibility in the component selection (the base ingredient as well as the fillers), and lower toxicity in comparison to the lead (Pb)-based ones. In this study, we manufactured paraffin-based composites with different concentrations of iron-encapsulated multi-walled carbon nanotubes (Fe@MWCNTs) (10 and 20 wt%), which were prone to shape change at average room temperature. Long Fe@MWCNT arrays were synthesized by catalytic chemical vapor deposition (c-CVD) using a saturated (at 293.15 K) toluene solution of ferrocene (FeCp2) (9.6 wt%) as a feedstock toward the highest efficiency for a complete Fe-encapsulation. The experimental data indicate that the shielding properties against gamma- and X-ray radiation are influenced by the filler concentration – the higher CNT content resulted in a greater ability to attenuate incident ionizing radiation. Finally, Fe@MWCNT–paraffin composites demonstrated corrosion resistance, as they did not react with 1 M aqueous solutions of NaCl, NaOH, and HCl.
Fig. 1 The most common applications of gamma and X radiation showed as a simplified scheme, which confirms the versatility of the utilization of these types of radiation in various areas including science, medicine and industry as the main ones. Adapted with permission from ref. 1, under RightsLink license number 5751940607057. |
Nevertheless, traditional X-ray and gamma-ray shielding materials rely on utilizing materials with high density, mainly lead (Pb), which is a serious threat to humans health.10 It is also worth mentioning the presence of other drawbacks such as weight, impracticality, difficult recyclability, and limited accessibility or ability to be produced in desired shapes.11,12 In order to overcome these limitations and achieve desirable physicochemical properties in addition to the maximum radiation dose suppression, numerous efforts have been made to enhance conventional solutions through the introduction of nano- and microcomposites. Nano- and microcomposites, as a relatively-new class of materials, due to their wide range of choice concerning the main ingredient (the continuous phase), fillers (nano- and micropowders), and other additives (e.g. plasticizers),1,13 gain an advantage over the current (i.e. frequently outdated) solutions, as the choice of matrix (with eventual modifier agents) and filler compounds is specifically selected for a clearly-determined application. The compound selection is usually established keeping in mind factors such as: emitted energy level, determination in terms of fixed/movable destination, elimination of a secondary radiation and durability to destructive ionizing radiation effects to mention a few fundamental ones. Having such knowledge, the selection of particles (bearing in mind the morphology in terms of size, type, specific surface area, purity, presence of surface modification, etc.) along with main compound guarantee meeting the physicochemical property expectations of such a developed shield. And so, Li et al.14 developed composites based on natural leather with coimpregnated Bi2O3 and La2O3 nanoparticles to accomplish a lightweight, flexible, and wearable X-ray shield, where minimization of secondary radiation was realized by the additional Bi2O3 coating at the bottom. As another example, Tekin et al.15 verified theoretically (using Monte Carlo simulation) the size influence of tungsten oxide (WO3) particles on the shielding properties of a conventional shield – concrete. A similar study was developed in ref. 16 where the topic of filler size was analyzed on ilmenite–limonite (ILC) concretes filled with WO3 and PbO particles (50 μm and 50 nm defined diameters) using a simulation approach. Finally, a study where the developed nanocomposite included more than one added filler (for instance boron nitride and graphene nanosheets in the polyester matrix17) could also be found. One should not forget that the utilized matrices sometimes are recycled ones, which proves that the scientific world bears in mind the problem of continuously growing waste amounts and remains on alert to partially prevent environmental pollution.18–21 More importantly, the inclusion of nano- and microparticles in the composition not only reduces the amount of raw materials but also allows for choosing the elements which are safe for the human body, exhibiting low toxicity and mutagenicity, among other factors.22,23
Focusing on the fillers, among nano-sized materials carbon nanotubes (CNTs) deserve special attention due to their light weight, high specific surface area, and excellent mechanical, thermal and electrical properties, accompanied by corrosion and oxidation resistance.24–26 Their particular properties depend on their morphology: diameter, length, shape (e.g. straight, waved, coiled, and branched27), the number of rolled-up graphene sheets (multi-walled or single-walled, MWCNTs or SWCNTs), as well as the presence of additions on their surface (covalent and non-covalent functionalization).28,29 Their potential use in the design of protective materials against X and gamma radiation has already been noticed, as a review paper30 reports, and included as a component of shielding materials. Remaining in the shielding field, one should not forget utilization of carbon nanotubes as microwave absorbers and electromagnetic interference (EMI) shields.24,31–33
Verma et al.34 developed an X-ray shielding nanocomposite, where bismuth(III) oxide (Bi2O3) were incorporated on MWCNTs (20–25-μm-long) and along with proper additions resulted in a material in the form of a gel, which was then spread on previously washed, and mechanically rubbed cotton fabric. The shielding bandages had the following dimensions: 60 cm in length, 10 cm in width, and 5 mm in thickness, and were examined on a Nomex Multimeter from PTW with X-ray photons of 50–80 kVp energies, for 200 ms at 100 mA. The study involved three varying bandage samples: untreated bandage, bandage treated only with MWCNTs, and one combining Bi2O3 and MWCNTs. The highest X-ray absorption was recorded for the third bandage sample, so the study was extended to verify the effect of the Bi2O3 nanoparticles’ concentration (70, 75, and 80 wt%) on the shielding properties. Clearly, the results indicated that the higher content of Bi2O3 nanoparticles improved the X-ray shielding properties. In another study,35 the X-ray attenuation efficiency of SWCNTs, MWCNTs, single-wall carbon nanohorns (SWCNHs), fullerene (C60), graphene oxide (GO), and a fabric-textile with a MWCNTs addition was developed, and compared to the highly oriented pyrolytic graphite (HOPG). The sample textile was manufactured with polyester fibers (0.19 mm in thickness) with 8 wt% of MWCNTs containing 2.5 wt% of TiO2. The disc-shaped samples (apart from HOPG), 13 mm in diameter, were examined using a monochromatic incident X-ray beam of MoKα (λ0 = 0.7107 Å) at 50 kV, and 10 mA (and 300 mA for the thickness-dependence study). Considering the mass attenuation coefficient (μm) values, the X-ray attenuating ability (50 kV, 10 mA) of the SWCNTs, MWCNTs, SWCNHs, and the fabric-textile with MWCNTs addition were superior in comparison to HOPG. The investigation also included the dependence of the X-ray attenuation ratio on the thickness of the textile sample. It was shown that the attenuation efficiency increased with the thickness, i.e., for a thickness of 24 mm, the attenuation was higher than 70%. Altarawneh et al.36 proposed a mixture composed of gelatin (gelatin from bovine skin type B) and distilled water as a matrix for MWCNTs (with 10–20 μm length and outer diameter 30–50 nm), or activated carbon, which were added in various concentrations: 0, 5, and 10 wt%. The mass attenuation coefficients of the synthesized samples were determined using a cesium source (137Cs, 662 keV energy) along with a sodium iodide (NaI) detector, where the experimental data was collected for 90 min, and compared to the theoretical values predicted by the XCOM program (at energies 1 keV–100 GeV). The authors demonstrated that samples with the MWCNTs addition attenuated slightly more efficiently than those with activated carbon: for 5 wt% addition, the experimentally-designated mass attenuation coefficient values were found as 0.079 ± 0.001 and 0.082 ± 0.001 cm2 g−1 for activated carbon and MWCNTs, respectively. Overall, the authors recommended using MWCNTs as the addition to shielding composites in the X-ray energy range (rather than in the gamma range) as the stronger interaction appeared when the wavelength of the radiation was near to the interlayer spacing of MWCNTs. The shielding performance of CNT films using 241Am (59.5 keV) and 137Cs (661.7 keV) was also determined.37 The CNTs contained 3–8 tube walls with declared 7.8 nm average diameter. The CNT films were synthesized using a floating catalyst chemical vapor deposition growth technique, and one layer of this film was about 10-μm-thick. The investigation involved an analysis of a random film, aligned film (15% stretching ratio), and resin-impregnated film (with added 35 wt% epoxy resin) with various numbers of layers: 150, 300, 450, and 600. Considering 59.5 keV energy (for the 241Am source), the highest mass attenuation coefficient was found for the second sample, i.e., the aligned film, and it was 0.6707 cm2 g−1, while for the random one and resin-impregnated film, the corresponding values were equal to 0.5894, and 0.3051 cm2 g−1, respectively. Those values were compared to the ones for aluminum, iron, copper, and lead. Considering the beam energy of 661.7 keV, the mass attenuation coefficient was higher for the random and aligned film than for aluminum, iron, and copper. Furthermore, Huang et al.38 manufactured silicone foams with various contents of oxidized MWCNTs (o-MWCNTs): 1, 5, 10, 20, and 30 wt% using solution casting, foaming and cross-linking reactions, in order to verify their gamma radiation stability. The thickness of composites varied from 0.5 to 6.4 mm. The composites were placed into a glass tube and exposed to the 60Co source radiation with the doses from 100 to 500 kilogray (kGy). The results showed that electromagnetic interference (EMI) shielding effectiveness (SE) was nearly unaltered considering a low content of o-MWCNTs (1 and 5 wt%), however, a slight decrement was noticed for the samples with 20 and 30 wt% addition when the absorbed doses increased from 100 to 500 kGy. In another study39 coupled semiconductor metal oxide (CSMO) nanocomposites were prepared using a powder metallurgy method, where different concentrations (1, 2.5, and 5%) of CSMO, including Fe2O3, TiO2, and CdO, were individually added to the ZnO–MWCNT composite. Additionally, the gamma-ray shielding ability was designed theoretically, using the MCNPX Monte Carlo code approach for the energies: 0.1, 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.8, and 1 MeV. The data confirmed that increasing energy caused a decrease in the linear attenuation coefficient (μ) value. Nevertheless, the highest linear attenuation coefficient value (and, thus, the lowest half-value layer) was revealed for the composite with 5 wt% addition of CdO for all gamma-ray energies. Interestingly, effects of the ionizing radiation on the properties of composites with the addition of CNTs (or only CNTs40) were also studied,41–43 where it was stated for instance, that the exposure to gamma irradiation did not meaningfully change the value of the glass transition temperature,41 enhanced the bonding and distribution of nanofillers within the matrix,42 and caused higher crystallinity of the nanocomposite.43 Interestingly, considering the second of the mentioned, one could not forget that a crosslinking reaction could be conducted using gamma radiation, thus eliminating the need to include other chemicals in this process.44,45
Despite the above-presented studies on the development of gamma- and X-ray shielding CNT nanocomposites, this field has not gathered adequate attention, indicating a requirement for further comprehensive exploration. This applies to both narrowed down data concerning matrix selection, as well as interest in modifying nanotubes as fillers to achieve superior gamma and X-ray attenuation (e.g., metal encapsulation or MWCNTs surface functionalization with heavy metal compounds). On the other hand, the ease of shaping shields would allow for a customization to various devices, installations, or materials, thereby increasing the effectiveness of protection against the ionizing radiation. Furthermore, it could be perceived, that there is an emerging trend focusing on the development of flexible nanocomposites as this feature undoubtedly positions them as a superior option compared to the conventional solutions.14,46–49 Such shielding nanocomposites could be tailored to the specific needs and requirements, ensuring the optimal safety measures. It is worth noting that the ability to easily-mold shields paves the way to the more innovative solutions in the field of nuclear energy. Indeed, modern shields could be designed to minimize radiation risks and enhance safety in the nuclear power plants. This, in turn, could contribute to the development of more advanced nuclear technologies that are both energy-efficient and environmentally safe.
The demand for personalized shields seems to be particularly high in the medical sector. Easily formable shields could be tailored to the specific anatomy of each patient, including adjustments for age, figure, and height. This customization would provide optimal protection of the surrounding body parts from harmful radiation exposure and would ensure meeting individual patient needs. Personalized, form-fitting shields could enhance patient comfort by reducing movement restrictions and providing a more secure and personalized experience during diagnostic and therapeutic procedures. Additionally, easily formable shield options have the potential to lower overall costs by avoiding the need for multiple shield productions based on individual patient anatomy, and consequently could reduce waste generated in the medical sector.
In our previous study,50 as shielding composites against gamma- and X-ray radiation we proposed shape-controlled paraffin-based composites with the addition of iron particles in nano- and microsizes. Iron, as a common and non-toxic element, could be undoubtedly considered as the first-choice filler in the shielding composites; however, CNTs could be considered superior for several reasons. Analyzing their shape and large surface area, the probability of interactions occurring – e.g. multiple-scattering interactions due to surface modification of MWCNTs through the presence of heavy elements as discussed by Verma et al.34 thus contributing to the improvement of the shielding property – with incident radiation seems to be greater in comparison to the dispersed individual iron particles. The designed composites should be characterized by stability and durability under the given conditions, thus, one should emphasize that CNTs also exhibit chemical resistance. This characteristic makes them suitable for the more stringent conditions (e.g., with high levels of humidity), where iron particles would undergo corrosion, which could lead to further degradation and weakening of the composite material. Last but not least, the light weight is also a factor considered in the design of shielding composites. Analyzing the density value, CNTs exhibit a lower density compared to iron.
Referring to the aforementioned information, that is on the one hand exploring a non-toxic filler with enhanced shielding capabilities and preserved corrosion resistance, and bearing in mind the scientific focus (concerning radiological protection) on the among others development of flexible shielding nanocomposites, we have manufactured shielding paraffin-based nanocomposites with the addition of Fe@MWCNTs, composed of 9.6 wt% Fe and long MWCNTs (douter = 54 ± 31 nm, l = 300 μm). Such an Fe-content represents the upper limit of iron phases encapsulation within the nanotube core governed by the maximum solubility of ferrocene in toluene at room temperature (i.e. the liquid CVD feedstock). The chosen paraffin, as a chemically neutral matrix, was easily-formable to any shape by the pressure and warmth of hands. Additionally, the studied nanocomposites were simple in terms of composition, i.e. only paraffin and Fe@MWCNTs, without the addition of plasticizers or other modifiers. The rationale behind the selection of those ingredients was their low toxicity, in comparison to the traditional lead covers, straightforward processability and recyclability due to the unlimited number of the desired shapes within the range of high performance.
The Fe@MWCNT–paraffin nanocomposites were manufactured using the cold mixing method. Firstly, the appropriate amount of Fe@MWCNTs and the neat paraffin were weighted on an analytical balance WTC2000 (Radwag, Radom, Poland). Subsequently, the samples were placed in a vacuum dryer Goldbrunn 450 (Berlin, Germany) at 393.15 K, i.e., a temperature above the melting point of paraffin, to remove the residual air. The final step, after the paraffin crystallization, was cold mixing on the previously designed hand press for ca. 50 min. Since the shielding properties were measured as a function of the thickness, the composites were placed in 2-cm-high rings. The final samples were prepared at two mass concentrations: 10 and 20 wt% (as a greater Fe@MWCNTs amount would not allow for obtaining the required composite's property – the easy formability provided with the warmth and force of hands), while no plasticizers were used to prepare the nanocomposites. A more detailed description of the manufacturing process (pictures of the manual press, an arrangement of three molds to ensure filling rings in photographs and designs) could be found elsewhere.50
UV-Vis spectra were obtained with a Hitachi U-2910 spectrophotometer from 280 to 1100 nm with 800 nm min−1 scan speed. A pure solvent cuvette was placed in the reference channel and a double beam mode was used. Measurements were performed using 10 mm quartz cuvettes. Samples were prepared by submerging paraffin composites (100 mg) in an acetic acid/hydrogen peroxide/sulfuric acid mixture (acetic acid 99.5–99.9% pure p.a. POCH (Poland), hydrogen peroxide solution 30% pure p.a. Chempur (Poland), sulfuric acid 96% pure p.a. Stanlab (Poland)) with a respective volume ratio (5/5/0.1 mL). Composite materials were left in solutions in a glass vial for one month. After this period, 3.5 mL of solution was taken for UV-Vis measurement.
The “mAs” designation is a parameter that is the product of the anode current and the exposure duration. It should be remembered, that its increase results in an increase in the patient's dose. The assumed (selected) mAs value could be obtained by changing the ratio of current to exposure time. The design of X-ray machines allows for the regulation of these parameters within a wide range. This is essential when selecting the operating conditions of the X-ray tube for the anatomical region being examined. More importantly, an incorrectly selected ratio of current to exposure time (even with the correct mAs product) might lead to the diagnostic errors. This is particularly important in imaging, e.g. the chest, where the minimum possible exposure time and high anode current are required to minimize undesired motion artifacts.
For the data acquisition, a digital detector, produced by AGFA (Mortsel, Belgium), was used. The images, stored in accordance with the DICOM standard, were not subjected to any postprocessing. The calculations utilized numerical values obtained from the detector, which represented the intensity of X-ray radiation that reached the detector after passing through the sample. The digital values within individual fields (neat paraffin, 10 and 20 wt% Fe@MWCNT composites, and without any sample – the aerated field) were read using MATLAB software (produced by The MathWorks, Portola Valley), where the ROI (Region of Interest) field was a square area of 50 × 50 pixels. The X-ray shielding ability was designated as the ratio of the signal intensity obtained from a specific thickness of the sample layer, Ilayersample, to the signal intensity for the aerated field, Iair, according to eqn (1) below:
(1) |
The wrinkled surface of the neat paraffin (Fig. 2b) and the corresponding composites (Fig. 2c and d) obviously corresponded with their macroscale plasticity (bendability and kneadability), which is important from the perspective of future application in the X- and gamma-ray shields. The Fe@MWCNT content positively correlated with density of the brighter surface spots. Importantly, the Fe-based phases, even for the 20 wt% Fe@MWCNT-based composites, were undetectable by EDX spectroscopy (Fig. S2, ESI†). This outcome confirmed the formation of the paraffin shell on every and each Fe@MWCNT nanoagglomerate in the final composites. The double shell, i.e., nanotube wall and paraffin, emerged as effectively shielding the Fe-core. Importantly from the viewpoint of corrosion resistance and iron (and other possible actively shielding components) leakage, no reaction with the corroding environments, such as 1 M HCl(aq), 1 M NaCl(aq), and 1 M NaOH(aq), also in the presence of the addition of 30 wt% H2O2(aq) as 1/3 of the final volume of the tested mixture, was detected (Fig. 3). This behavior was opposite to the only-Fe paraffin composites50 which underwent a progressive digestibility.
Fig. 4 Differential scanning calorimetry (DSC) curves for neat paraffin (green) and its 10 wt% (blue) and 20 wt% Fe@MWCNT (red) composites. |
At the same time, the decrease in the enthalpy of solidification was found to be practically directly proportional to the Fe@MWCNT content as the latter is a stable-phase solid component: the expected values of the solidification enthalpy for 10 wt% and 20 wt% Fe@MWCNT would be 16.0 and 14.2 J g−1 while the actual values were found to be 16.2 and 14.0 J g−1. Further, to study the thermal resistance of Fe@MWCNTs, paraffin, and their composites, TGA – both combustional (Fig. 5B) and pyrolytic (Fig. 5A) – was performed. Pyrolytic TGA, confirming the Fe-content in Fe@MWCNTs, showed that incorporation of Fe@MWCNTs led to an increase in the thermal stability of the composites. This increase in thermal stability under the inert atmosphere would be a result of trapping alkyl and oxygen radicals by Fe@MWCNTs of a higher specific surface area.60
Fig. 6 Fourier-transform infrared (FTIR) spectra of Fe@MWCNTs (black), paraffin (green) and their 10 wt% (blue) and 20 wt% (red) Fe@MWCNT composites. |
In order to employ a paraffin composite filler of the potentially highest shielding efficiency, we have synthesized Fe@MWCNTs using the saturated solution (at 293.15 K) of FeCp2 in toluene (9.6 wt%) as the feedstock. Such an approach led to a total-Fe-encapsulation efficiency at the level of 10 wt% (as previously determined by TGA). Concerning analysis of the micromorphology, optical micrographs of neat paraffin, Fe@MWCNTs, and their composites (Fig. S1, ESI†) showed a partial conservation of the aligned, fibrous-like nature of Fe@MWCNTs in the composites, with different levels of the nanotube agglomeration. More importantly, samples developed in the previous study50 as well as the ones with the addition of Fe@MWCNTs were treated with a strongly aggressive medium composed from H2O2(aq) (30%), CH3COOH (99.5%), and H2SO4(aq) (96%), (v/v/v = 5:5:0.1). The rationale behind this experiment was as follows: if the iron phases would be present exohedrally (anchored to the outer nanotube shell), the immediate reaction of FeOOH (constituting the shell at ambient air temperature) should occur61 generating Fe2+ ions immediately oxidizable to Fe3+ ions62 and further transferred to the strongly acidic bulk digesting solution. While, the UV-Vis spectra developed after one month in the aggressive medium confirmed that samples with the Fe@MWCNTs addition had not experienced a gradual increase in digestibility (Fig. 7). This behavior was opposite to the only-Fe paraffin composites50 which underwent a progressive digestibility (Fig. 7), thus confirming that composites with Fe@MWCNTs would be more suitable in terms of not releasing into the human organism.
Fig. 7 Ultraviolet–visible light (UV-Vis) spectra of samples treated by a strongly aggressive medium composed from H2O2(aq) (30%), CH3COOH (99.5%), and H2SO4(aq) (96%), (v/v/v = 5:5:0.1) recorded after one month: neat paraffin (green), 10 wt% Fe@MWCNTs (blue), 20 wt% Fe@MWCNTs (red), Fe–paraffin from ref. 50 (orange). |
Results of experimental investigation of the rheological properties of Fe@MWCNT-paraffin composites are presented in Fig. 8 and 9. The dependence of the values of the storage (G′) and loss (G′′) moduli on the deformation at constant temperature 309.75 K are presented in Fig. 8 and listed in Table S1 (ESI†). It could be noted that the developed nanocomposites were stable for low deformations, up to 0.1%, and the critical deformation is higher than that noted for pure paraffin (∼0.05%). It has been shown that the proposed nanocomposites could be easily formed with bare hands, which is an undoubted improvement over the standard used lead shields.
Findings of the temperature sweep in the temperature range from 288.15 to 338.15 K, at a heating rate of 0.5 K min−1, where the strain was set to 0.01% at frequency equal to 1 Hz are presented in Fig. 9, and summarized in Table S2 (ESI†). As expected, the values of G′ and G′′ decrease with temperature, however, one could note that in the nanocomposites viscoelastic structure could be consider as stronger.
The rheological experiments included an amplitude sweep at 309.75 K with a frequency equal to 1 Hz, as well as a temperature sweep in the temperature range 288.15 to 338.15 K, at a heating rate of 0.5 K min−1, where the strain was set to 0.01% at a frequency equal to 1 Hz. Tables S1 and S2 (ESI†) contain experimental values of the storage modulus and loss modulus for the pure paraffin as well as Fe@MWCNT-paraffin composites (at various concentrations) for both of the rheological characteristics.
N = N0e−μx, | (2) |
(3) |
(4) |
In this study the linear attenuation coefficient μ (cm−1) was experimentally determined by fitting an exponential curve to the experimental data as the modeled equation (eqn (5)) shows:
(5) |
In this study, gamma-ray shielding properties of the manufactured composites were determined considering two different Fe@MWCNT mass concentrations. The obtained results are presented in Fig. 10, while the precise data is included in Table S3 (ESI†).
Fig. 10 Ratio of the number of detected photons in the G–M counter for each of the examined layer thicknesses (from 2 to 26 cm with a 2-cm-step) versus the number of photons collected without any layer on the paraffin-based composite thicknesses with 10 wt% and 20 wt% addition of Fe@MWCNTs. The symbols and lines represent the experimental and eqn (5) fitting data, respectively. |
Based on the acquired data it could be noticed, that the addition of Fe@MWCNTs had slightly improved gamma shielding properties in comparison to the pure paraffin. The summarized linear attenuation coefficients, together with the half value layer data included in Table 1, also demonstrated this relationship.
Sample | μ (cm−1) | HVL (cm) | MFP (cm) |
---|---|---|---|
Paraffin | 0.04550 ± 0.00047 | 15.23 ± 0.31 | 21.98 ± 0.45 |
Paraffin + 10 wt% Fe@MWCNTs | 0.04925 ± 0.00050 | 14.07 ± 0.29 | 20.30 ± 0.41 |
Paraffin + 20 wt% Fe@MWCNTs | 0.05195 ± 0.00044 | 13.34 ± 0.23 | 19.25 ± 0.33 |
And so, when analyzing the HVL values, it could be observed that the paraffin thickness of ca. 15 cm absorbs half of the incident radiation beam, whereas for the composite with a 20 wt% addition of Fe@MWCNTs ca. 13-cm-thickness is required. Fig. 11 presents the bar graph with the HVL values of neat paraffin versus its composites, where a decrease in HVL after the addition of nanotubes is visible. The shielding effectiveness, as a result of greater Fe@MWCNTs amount, could be noticed in terms of the MFP (cm) factor (Table 1), where its value decreases analyzing pure paraffin and paraffin + 20 wt% Fe@MWCNTs composite.
Fig. 11 Half value layer (HVL) of the manufactured Fe@MWCNT–paraffin composites, and pure paraffin presented in the single bars confirming the HVL value decrease with higher Fe@MWCNTs content. Table 1 provides the specific HVL values, along with their corresponding uncertainties. |
It could be observed that the scientific literature discusses the impact of filler concentration on the shielding properties of composites. Therein, a majority of the studies confirmed that a higher content of nano- and micromaterials improved the shielding ability.67–69 Our studies also confirmed the above data, i.e., μ values for the composites – filled with 10 and 20 wt% of Fe@MWCNTs – were found to be equal to 0.04925 and 0.05195 cm−1, accordingly. Focusing on the μ-values, in comparison to the pure paraffin the linear attenuation coefficient of paraffin + 20 wt% Fe@MWCNTs was ∼14% higher, thus confirming that Fe@MWCNTs addition has successfully improved the shielding ability of the matrix. Despite the fact that lead (as the traditional and commonly utilized gamma shield) has superior shielding properties (considering simulation-determined linear attenuation coefficients for lead were μ = 0.694 ± 0.002 and μ = 0.625 ± 0.002 cm−1 accordingly corresponding to two gamma energies emitted from 60Co: 1773 keV, and 1332 keV70) in comparison to the developed paraffin + Fe@MWCNTs composites, it should be emphasized that the latter could be characterized as a non-toxic shield option with versatility in shape definition provided simply with the warmth and force of hands – features that cannot be attributed to the strictly-determined shapes of Pb-based covers.
Focusing on the shielding mechanism, the photoelectric effect, Compton scattering and electron positron pair production should be named as the three mainly occurring phenomena in the case of gamma rays interaction with matter – the γ-ray energy (MeV) and the atomic number of the material (Z) determine which effect dominates.71 In the current study, considering the used fillers (Fe@MWCNTs) along with the utilized source (60Co, ∼1 MeV energy), the Compton effect – inelastic scattering of the incident beam on electrons (whose binding energy is much smaller than the energy of the incident radiation beam), where as a result of this phenomenon the electron is ejected and the remaining photon with a lower energy changes the direction of its propagation (in accordance with the principle of conservation of energy and momentum) – seems to be the most probable for the shielding mechanism.72,73
The basic law that presents the attenuation of incident X-rays after interaction with shields could be formulated as:
(6) |
The linear attenuation coefficient determined for the Fe@MWCNT–paraffin composites, and neat paraffin, was established by a fitting modeled equation to the experimentally-obtained data:
(7) |
The experimental data, together with the fitted curves (eqn (7)), are depicted in Fig. 12, while the μ values for paraffin, nanotube composites (along with calculated HVL, MFP values) are summarized in Table 2.
Fig. 12 Dependence of the X-rayattenuationfactor−1 for different thicknesses (2, 4, 6, and 8 cm) for the pure paraffin and paraffin-based composites with 10 wt% and 20 wt% addition of Fe@MWCNTs at the 70 kV anode voltage. The symbols present the experimentally-achieved data, while the lines present the eqn (7) fitting data. |
Sample | μ (cm−1) | HVL (cm) | MFP (cm) |
---|---|---|---|
Paraffin | 0.1795 ± 0.0020 | 3.861 ± 0.086 | 5.571 ± 0.124 |
Paraffin + 10 wt% Fe@MWCNTs | 0.1997 ± 0.0016 | 3.470 ± 0.056 | 5.008 ± 0.080 |
Paraffin + 20 wt% Fe@MWCNTs | 0.2152 ± 0.0040 | 3.220 ± 0.120 | 4.647 ± 0.173 |
It could be stated that the increasing Fe@MWCNT content contributed to the X-ray shielding ability improvement: the HVL-values of the neat paraffin and 20 wt% Fe@MWCNTs were 3.861 and 3.220 cm, respectively. The superior X-ray attenuation could be noticed in composites with greater Fe@MWCNTs amount in terms of MFP factor, as the lower MFP value confirms improved shielding properties. Again, the literature reports a similar trend, where greater filler amount influenced the MFP value decrement.74–76
Here, we have designed, developed and elaborated shielding composites based on paraffin with the addition of Fe@MWCNTs (at concentrations of 10 and 20 wt%), which were tested for their shielding abilities against gamma- and X-ray radiation. The developed composites were characterized by their simplicity of composition (where only two components were utilized), with a commonly available, ready-to-use, chemically inert and inexpensive matrix. The Fe@MWCNT filler allowed for the development of a non-toxic composite (Pb-free), and its addition has successfully enhanced the shielding properties of paraffin due to the combination of MWCNTs with an encapsulated metal (Fe) compound inside. The conducted research confirmed the dependence of the shielding capability on the amount of the added Fe-encapsulated nanotube filler. More importantly, as the outcome of the studies on the behavior of the paraffin + 20 wt% Fe@MWCNT nanocomposites under harsh, corroding conditions presents the individual ingredients will not be released into the human body and the environment. It should be also noted that the final composites featured a simple processing (without any need for highly specialized equipment), and minimalism in terms of composition. This leads to a reduction in the production time and cost, energy savings, and, more importantly, availability to a broad spectrum of researchers, industry and medical workers, and material engineering designers (especially including radiological protection). Although the proposed nanocomposites have a weaker ability to attenuate radiation than pure lead, due to their advantages such as low density, non-toxicity and ease of formation, they could be an alternative to these classic radiation protection materials. Summing up, it has been shown that the use of nanotubes significantly reduces susceptibility to corrosion and increases the stability of nanocomposites, which is crucial keeping in mind durability and the multi-aspect nature of the working conditions.
Bearing in mind the susceptibility of Fe@MWCNT-paraffin composites in terms of shape definition at average room temperature under pressure and heat from the hand touch it should be stated that such a solution overcomes a challenge where manufacturing complex traditional covers is impossible or shape changes could not be developed to a satisfactory degree (thus requiring the repetition of the manufacturing procedure). The developed Fe@MWCNT-paraffin composites could be implemented in various areas of our every-day life research and scientific facilities, i.e., as: (1) a supportive element in the shielding constructions, (2) adjusted containers for radioactive waste transport, (3) personalized shields for patients in hospitals (e.g., to protect sensitive areas of the body during X-ray imaging), (4) for workers exposed to ionizing radiation (e.g. in the nuclear energy sector), and (5) to shield, and maintain undisturbed working of sensitive electronic equipment placed in areas of radiation exposure.
This study identifies a few gaps; therefore, the following potential future directions are outlined. Firstly, development of the composites, including CNTs, could be recognized as remaining in the early stages of progress (as they have not received wide attention as in the case of heavy particles1), the research should be continued with insight into the X and gamma-ray attenuating properties of nanotubes varying in morphology. This includes combinations of the number of walls (SW- or MWCNTs), the potential influence of the concentration of the encapsulated compound (if any) inside the carbon nanotubes, and the presence of periodically distributed heavy metal compounds on the nanotube surface (including pure nanoparticles such as Pb, W, Bi, etc., as well as their compounds/oxides), among other factors. As alternatives, since MWCNTs could be synthesized via c-CVD from various (non-)metallic precursors,77–81 other nanoparticle@MWCNT systems could be used as equally or even more promising fillers. Comparative shielding tests between commercial CNT products and those laboratory-synthesized should not be omitted. The various orientations of carbon nanotubes (again, considering variety of CNTs morphology) should be analyzed more comprehensively to understand their impact on the shielding properties of the developed composites.82 Maintaining versatility in matrix selection is also crucial as it not only provides a comprehensive overview of real-world shielding nanocomposites implementation possibilities but also facilitates the creation of databases essential for developing theoretical models. Considering the unique mechanical properties of carbon nanotubes along with variety in terms of matrix selection it is essential to not only determine the shielding properties (X, gamma), but also to evaluate the rheological properties of the developed shielding composites. Moreover, other studies should be added reflecting the durability aspect (the effect of gamma or X-rays on the composite in terms of damage), and the examination of gamma-ray shielding properties should be included over a broader energy range (using other sources). Finally, as carbon nanotubes are recognized for EMI shielding and microwave absorption,83,84 while paraffin is for neutron shielding, the developed hybrid paraffin + Fe@MWCNTs composites could be examined in these two areas to verify additional (diverse) attributes.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ma00359d |
This journal is © The Royal Society of Chemistry 2024 |