Open Access Article
Shuanglin
Zheng
a,
Wenjuan
Bian
b and
Hanping
Ding
*a
aSchool of Aerospace and Mechanical Engineering, University of Oklahoma, Norman, OK 73019, USA. E-mail: hding@ou.edu
bDepartment of Hydrogen and Electrochemistry, Idaho National Laboratory, Idaho Falls, ID 83415, USA
First published on 14th February 2024
Developing protonic ceramic fuel cells is regarded as a promising approach for the electrochemical conversion of the chemical energy in hydrogen to power with high efficiency. Lowering the operating temperature can accelerate its application by integrating more reliable stack components to enable long-term durability. One critical pathway is to facilitate the oxygen reduction reaction via developing triple conducting oxygen electrodes for increasing active sites for catalysis and charge transport in bulk and interface, aiming to improve reaction kinetics. In this work, the recently developed triple conducting oxygen electrode PrNi0.7Co0.3O3−δ has been examined under dynamic operating conditions to understand the degradation behaviors through an accelerated stress test. Various test protocols have been employed to measure and compare the mechanical and electrochemical performances under different dynamic parameters and thermal cycling conditions. The results strongly indicate that the as-fabricated cells exhibit a high level of endurance despite a slightly increased polarization resistance and an accelerated stress test is an effective way to examine cell reliability under more dynamic kinetics.
As reducing operating temperature can significantly improve material compatibilities and cost-effectiveness of stack manufacturing, considerable endeavors have been made to enhance the performance of materials in the temperature range of 400 °C–600 °C and ensure their long-term stability.16–19 However, the sluggish reaction kinetics of oxygen electrodes leads to the remaining technical challenges in pursuit of suitable electrode compositions for the water splitting reaction. To overcome this rate-limiting step, developing a triple conducting electrode is considered as an effective approach to extend active reaction sites throughout the entire electrode surface and interface for accelerating the kinetics of oxygen evolution and proton transfer.20–23 There have been several examples of triple conducting oxide (TCO) materials being developed, demonstrating significant proton conductivity and improved cell performance by increasing the reaction efficiency of both the hydrogen oxidation reaction (HOR) and the oxygen reduction reaction (ORR) at triple phase boundaries (TPBs).24–27 PrBa0.5Sr0.5Co2−xFexO5+δ (x = 0, 0.5 and 1.0), one promising layered perovskite, was compounded to promote electrochemical active sites, realizing lower area specific resistance (ASR), 0.33 Ω cm2 at 500 °C and 0.056 Ω cm2 at 600 °C, than Ba0.5Sr0.5Co0.8Fe0.2O3-δ at similar temperature (0.70 Ω cm2 at 500 °C).24,25 These doped variants demonstrated the intensified oxygen bulk diffusion and surface exchange. BaCo0.4Fe0.4Zr0.1Y0.1O3−δ, another TCO material, was based on a material family of proton conducting electrolytes with intrinsic proton formation properties, resulting in a significant improvement in the overall performance of the cell.26–28 Some other examples also include a group of unique La–Ni based layered perovskites, recognized as Ruddlesden–Popper oxides, Lan+1NinO3n+1, being selected as an alternate material for the cathode. Pr1.75Ba0.25NiO4+δ and Pr1.2Sr0.8NiO4+δ, with different substitution at the A-site, both exhibited triple mixed conductivity. The dispersion of extra oxygen ions in the interstitials can enhance ionic transport, thus yielding oxygen exchange properties as well as hydration.29–32
We have recently demonstrated a perovskite-structured PrNixCo1−xO3−δ (PNC) oxide as a TCO oxygen electrode for electrochemical cells in the operation of a fuel cell or an electrolysis cell.33,34 This PNC electrode can function as the oxygen electrode (cathode) featuring high efficiency and stability, hence avoiding any need for doping with alkaline earth metals such as calcium, strontium, and barium for higher activity. Although the doping of these elements to increase the ionic conductivity and accelerate ORR kinetics is undebatable, the tendency for enrichment and segregation at interfaces often results in further exacerbation by the presence of carbon dioxide and water vapor. Moreover, a higher level of hydration ability makes the proton defect concentration significantly increased, which is a contributing factor to triple conduction. The density functional theory calculation also indicated the reduction of barrier energy favorable for proton conduction.35–39 This electrode has demonstrated excellent electrochemical activity for both the ORR and water oxidation reaction in fuel cell and electrolysis modes due to several factors: high oxygen vacancy concentration, highly triggered proton conductivity from the hydrated lattice, and low thermal expansion coefficient. After integration into BaZr0.4Ce0.4Y0.1Yb0.1O3−δ (BZCYYb4411) electrolyte based cells, it exhibited peak power density of 0.53 W cm−2 at 600 °C in the fuel cell mode and 1.31 A cm−2 at 1.40 V and 600 °C in the electrolysis mode respectively, which were ranked among the highest performances.40 In order to achieve a balance between activity and thermal properties, this material system has undergone additional optimization via the examination of a range of compositions regarding PrNixCo1−xO3−δ (x = 0.1, 0.3, 0.5, 0.7, and 0.9) with different Ni/Co ratios to find the optimal composition. It was revealed that PrNi0.7Co0.3O3−δ (PNC73) showed exceptional performance and adjusted thermal matching properties with the electrolyte. The electrolysis current density reached up to 1.48 A cm−2 at 1.3 V and a peak power density of 0.95 W cm−2 was achieved at 600 °C, exceeding the performance of the PNC55 electrode by 80%. This electrode also showed satisfactory output (0.14 W cm−2) when the temperature was reduced to 350 °C.33,34
To further validate the feasibility of this PNC73 electrode in a PCFC system, the evaluation of long-term stability in the operation mode is very critical, which is essential for scaling up and commercialization.41–44 The accelerated stress test is an effective method to examine the robustness of cell properties by challenging the adaptability of materials and interfaces upon dynamic changes of testing conditions. In this work, we have performed a series of accelerated stress tests on single cells with the BCZYYb4411 electrolyte and PNC73 oxygen electrode. Our results have preliminarily demonstrated that the electrochemical performances are robust against dynamical stress operations, which is attributed to the enhanced interface bonding strength.
Fig. 2a demonstrates the main comparisons of the electrochemical performance of the cell operating at 600 °C in the fuel cell mode with pure hydrogen as fuel after different transient test modes as shown later in Fig. 3. First, the open circuit voltage (OCV) of the cell is 1.08 V before any test, and 1.10 V after the step voltage test and transient voltage test, which are close to the theoretical potential value (1.13 V) calculated using the Nernst equation. This result proved that the electrolyte membrane is very dense and excellently sealed. Furthermore, the I–V curves yield no drastic non-linear fluctuation, confirming that the interior structure of lanthanide nickelates is little compromised. The peak power densities are 457 mW cm−2 before the test, 342 mW cm−2 after the step voltage test and 302 mW cm−2 after the transient test, respectively. Though peak power densities have been decreased by 33% and 51% in two distinguished stressed modes separately, they are still competitive among other cathode materials. More specifically, the performance (302 mW cm−2 at 600 °C after the transient test) has been approximately three times higher than the cell with selected rhombohedral phase La0.7Sr0.3Mn0.7Ni0.3O3−δ (LSMN7373) as the cathode (102 mW cm−2 at 600 °C) and similar to the peak power density of cubic phase LSMN7373 (386 mW cm−2 at 600 °C), which has been highlighted.51 More work related to other cathode components, such as (La0.6Sr0.4)0.95Co0.2Fe0.8O3−δ, consistently showed lower peak power density (214 mW cm−2 at 600 °C), all verifying the potent capability to maintain the efficient ORR activity occurring at the interface and substantial triple-conducting paths are preserved, then shedding light on the long-term cell use or operation under extreme electrochemical conditions.52 As indicated in the impedance spectra (Fig. 2b), though the ohmic resistance Ro has recognizable escalation, ranging from 0.13 Ω cm2 to 0.23 Ω cm2 and then increases to 0.34 Ω cm2 correspondingly, the polarization resistance Rp of each cell sample is close to 0.44 Ω cm2 (0.39 Ω cm2, 0.45 Ω cm2 and 0.48 Ω cm2, respectively), denoting no sharp increment and assuring that every layer of full cells has been well-functional with continuous current flowing. It should be noted that this temporary degradation on current density or polarization resistance will be relieved after the dynamic operation is terminated for a while.
For a detailed constant step-voltage test, the applied potential on full cells has been altered from 0.8 V to 0.6 V and then to 0.4 V, from high to low and then back forth with certain changing patterns, and the duration of each stagnant-voltage was 1 h, repeated for 17 cycles at unchangeable 600 °C (Fig. 2c). It is apparently noted that, when applied with potential 0.4 V for four intermittent cycles, the current density of each cycle has been clustered around 0.92 A cm−2 but also with the analytical fluctuation range of 0.14 A cm−2. Resembling tendency is witnessed while altering the applied potential to another two pre-set values, the current density converges at 0.38 A cm−2 for 0.8 V and 1.5-fold increased value (0.59 A cm−2) for 0.6 V. Additionally, the cell stability, in terms of step-voltage shifting, has been further substantiated through the mean value of current density for each cycling duration. For instance, the average current densities of four cycles at 0.4 V are 0.94 A cm−2, 0.96 A cm−2, 0.94 A cm−2 and 0.84 A cm−2 (green solid lines as indicated); comparably, the average values of eight cycles at 0.6 V are 0.79 A cm−2, 0.68 A cm−2, 0.64 A cm−2, 0.57 A cm−2, 0.54 A cm−2, 0.55 A cm−2, 0.50 A cm−2 as well as 0.49 A cm−2 (black solid lines as indicated), and the mean ones of five patterns at 0.8 V are 0.31 A cm−2, 0.34 A cm−2, 0.36 A cm−2, 0.42 A cm−2 and 0.48 A cm−2 (blue solid lines as indicated). The slightly downscaling current density is irrefutable under long time stressed tests due to oxygen starvation and possibly some stress-induced electrode interface deterioration.
Predominantly, the dashed trendlines in Fig. 2c also indicate the insignificant variation in cell performance for inconsistent voltage restrictions, resulting in exceptional durability under step-voltage conditions. When a 0.8 V input voltage was applied, the current density decreased marginally from 0.48 A cm−2 in the first cycle to 0.31 A cm−2 in the fifth cycle. Similarly, at 0.6 V and 0.4 V, the current density reduced to 0.49 A cm−2 in the eighth cycle and 0.84 A cm−2 in the fourth cycle, respectively. This non-equilibrium response is common to some degree, and it is not very clear to identify the certain reasons. However, it is indisputable that the current densities obtained even at the end of step-voltage tests approximately were close to 0.50 A cm−2, which was just over the cells using PrBa0.5Sr0.5Co2O5+δ as the cathode.53 The steady current density at high input voltage remained around 0.31 A cm−2, which is surprisingly higher than that of full cells using certain PNC series electrodes as PNC37 or PNC19.33 As shown in Fig. 2d and e, the constant-voltage cell stability test has been conducted for 20 h when the cell was fixed at 0.75 V and 600 °C and the related impedance spectrum has been collected. The result demonstrates the stable output under a steady condition instead of dynamic operation, which indicates that the dynamic operation is more useful to investigate the electrochemical behaviors.
The current density was initially 0.33 A cm−2, and then it has gradually ramped up to 0.42 A cm−2 after the fuel cell experienced electrochemical conditions for 11 hours though it slightly dropped to around initial value at the end of 20 hours duration. In terms of functioning time, the current density of the PNC73 full cell fluctuated around 27%, which holds its stability for long-term working conditions. It is also worth mentioning that the Ro is 0.22 Ω cm2 and Rp is 0.41 Ω cm2, which are more closely aligned with the values of the cell before the transient tests in Fig. 2b. Therefore, we can conclude that the dynamic operation challenges the cell stability significantly, which is essential for evaluating PCFC stability.
The PNC73 full cell was thereafter subjected to the transient test by sweeping among a range of voltages. As presented in Fig. 3a, the results of the transient cycling test for 100 cycles, when the applied potential on the cell was between 0.8 V and 0.2 V, provide the information that there is an evident horizontal shift towards left with more cycles conducted. This showed some slight cell degradation with decreased current density, especially by comparing the first five cycles with the last five cycles. It is attributed to oxygen starvation, which is not a permanent degradation. Furthermore, the initial current density for the first transient test at 0.8 V was 0.36 A cm−2, which definitely meets the criteria for downscaled performance in robustness testing. This was similarly observed for both 0.6 V and 0.4 V conditions. The subsequent results are derived from the comparison between the initial current density and instantaneously recorded values under each specific voltage and electrochemical conditions within the first transient test. When the applied voltage is regarded as the control variable, the maximum amount of variation in current density for 100 cycles is 0.09 A cm−2 for 0.2 V, while the minimum is 0.04 A cm−2 for 0.8 V. These findings confirm that the low applied voltage should be reduced in order to ensure the long-term durability of cells. After re-categorizing the I–V data, the results concerning four groups of 1st–25th, 1st–50th, 1st–75th and 1st–100th cycles are organized to display the analogous trend of cell performance on the mild downgrade (Fig. 3a–e). With each additional 25-cycle operation, the durability of the PNC73 full cell was further investigated. For instance, ar 0.6 V, the varying range of current density is 0.08 A cm−2 for the first 25 cycles, while that for the following three repetitions is 0.05 A cm−2, 0.02 A cm−2 and 0.01 A cm−2 respectively, indicating that the output amount is trimming but generally stable and achieves vital durability until the last cycle. Furthermore, the I–V relationship of each transient cycle, as shown in Fig. 3b–e, is confirmed to be roughly linear and steady, confirming the integrity of layered-structures and stable interfaces on cells and holding consistency with results from SEM images. Clearly, while linking a similar downscaling shift among 1st–5th cycles with 96th–100th cycles, the current density has decreased more drastically in the early stages of cycling than in the last few cycles. After explainable degradation proceeded, the cell performance tended to be determinate with certain sets of current density–voltage values, which was anticipated by previous electrochemical results.54–56
The step voltages applied have some negative effects on the full cell electrochemical performance, resulting in deterioration in current density. Later, we would discuss that these problems are temporary. Thus, the second transient cycling tests between 0.9 V and 0.2 V for 100 cycles in the fuel cell mode, but with different levels of applied voltages, 20 mV, 50 mV and 100 mV respectively, have been conducted. As shown in Fig. 4a–c, the comparison of the diminishing amount of current density (the horizontal shift on each curve) indicates that when the variation of step voltage was 100 mV, the ranges of current density were the largest, 0.06 A cm−2 for 0.2 V and 0.03 A cm−2 for 0.9 V. To clearly show one cycle, Fig. 5a shows the difference in current density at the same voltage, which indicates that the dynamic cycling would not easily yield the exactly same curves. In comparison, the ranges were 0.02 A cm−2 for 0.2 V and 0.03 A cm−2 for 0.9 V as the variation was 20 mV, whereas they were 0.02 A cm−2 for 0.2 V and 0.01 A cm−2 for 0.9 V as the variation was 50 mV. Although the result of degeneracy in cell performance is not negligible when the variation is 100 mV at 0.2 V and 600 °C, which is 0.06 A cm−2, the shifts of current density under other testing conditions are validated to keep up steady cell performance with continual current generated. Similarly, when focusing on grey dots representing other cycles in between, it holds consistency of the marginally dropping pattern on current density to the lowest level of the ultimate cycle almost for all three settings. However, it is obvious that several middle cycles yielded weaker performance at 100 mV step voltage, which seems unseen before, but the current density varied in a certain range highly elucidates this unique dynamic stability. These shifts are the temporary phenomenon due to the oxygen starvation when the current density is dynamically changed, and the cell was not damaged by these operations.
The impedance spectra were collected after each cyclic test in Fig. 4, as shown in Fig. 5b. The maximum of Ro (0.50 Ω cm2) belongs to the cell when the voltage change was 100 mV, followed by 0.32 Ω cm2 for 20 mV and 0.47 Ω cm2 for 50 mV, demonstrating that the larger shift of practicable voltage led to highly escalated ohmic resistance. However, the Rp of three testing procedures showed reverse pattern, that is, the Rp of the cell experienced changing voltage of 100 mV is the minimal 0.65 Ω cm2, and they are 0.79 Ω cm2 for 20 mV and 0.68 Ω cm2 for 50 mV. From these results it seems difficult to determine which modification has the least influence on cell stability, but when we relate the results of both resistances of after-transient cells to that of pristine cells (Ro = 0.13 Ω cm2, Rp = 0.39 Ω cm2), it can be clearly determined which transient or cycling thermochemical test influences the stability of PNC73 cells but the cells still function smoothly regardless of the degraded performance. Overall, when evaluating the constant step-voltage test, first transient test, and second transient test as a sequence of tests to assess the durability of PNC73 cells, it becomes evident that the critical electrochemical performance, specifically the current density, is prone to decrease unsubstantially between any two tests, including initial values as comparison. For instance, the current density at 0.6 V for the constant step-voltage test varied between 0.49 A cm−2 and 0.79 A cm−2. Similarly, during the first transient test and second transient test, the current density ranged from 0.44 A cm−2 to 0.54 A cm−2 and 0.45 A cm−2 to 0.54 A cm−2, respectively. However, the unanimous de-escalating performance of full cells is subjected to the working lifetime of any random cell. With the stabilized dropping range of 0.10 A cm−2–0.30 A cm−2, the PNC73 cells undoubtedly show durability under collective transient tests.
After these cyclic tests, an constant-voltage stability test was performed to collect the EIS spectra for comparing the evolving cell status. The temperature and voltage were set as 600 °C and 0.2 V. Taking two hours period as a cycle, by the comparison of nine ones, evidently, the current densities are all approximately at the same level, around 1.15 A cm−2, and no abrupt downfall of performance occurred. More importantly, the current density can achieve up to 1.17 A cm−2, which is clearly witnessed. Although there are countable outliers existing, larger or smaller than the mean value, the cell is in its overall stable condition. As impedance spectra can reveal (Fig. 6b), specifically, Ro and Rp of each cycle varied a little from others, gathering around 0.25 Ω cm2 and 1.23 Ω cm2 respectively, indicating the complicated dynamic status of the cell during the test. Only during last three periods, when the testing duration was between 12 and 18 hours, Rp mildly dropped (less than 10%), which might be explained by the enhanced triple-conducting path and the comparatively flawless gas environment to ensure the HOR and ORR with high-grade chemical kinetics.57–59
The thermal cycling resistance was examined by measuring I–V curves between 600 °C and 500 °C 10 times. Immediately after reaching the temperature point, the cell was scanned and the OCV at both temperatures reached around 1.10 V, proving that the fabrication and sealing are long-lasting for the varying temperature, as shown in Fig. 7.34 The result indicated that the I–V curves have very little variation among them as they are mostly overlapped. After excluding extraneous experimental conditions such as voltage, and when the temperature, which has been shown to have the dominant effect on cell performance, was used as a variable, a stable and certain current density, even the peak power density, has been achieved, which is the corroboration on the stability of PNC73/BZCYYb/NiO-BZCYYb fabricated cells.
![]() | ||
| Fig. 7 Thermal cycling examination: (a) I–V comparisons for 600 °C and 500 °C during the thermal cycling test. (b) EIS comparisons at 600 °C and 500 °C during the thermal cycling test. | ||
:
citric acid
:
cations = 1
:
1.5
:
1, with a cation concentration of 0.02 mol L−1. The initial precursor solution was subsequently heated while being stirred magnetically for hours. Once the viscous gel was formed, it was then subjected to additional heating at around 200 °C to achieve self-ignition. Ultimately, the gel turned to be a substantial amount of powdery ash. After being transported to a muffle furnace for calcination at a temperature of 1000 °C for 5 hours, the product was finally formed as a crystalline perovskite phase. The electrolyte powder, BaCe0.4Zr0.4Y0.1Yb0.1O3−δ (BCZYYb4411), was synthesized using a solid-state reaction (SSR) method. The stoichiometric amounts of raw chemicals BaCO3 (99.8%, Alfa Aesar), ZrO2 (99.9%, Alfa Aesar), CeO2 (99.9%, Alfa Aesar), Y2O3 (99.9%, Alfa Aesar), and Yb2O3 (99.9%, Alfa Aesar) were weighed and mixed in ethanol for ball-milling in planetary patterns at 300 rpm for 24 h. The powder product was then dried in an oven and calcined at 1000 °C for 5 h in the muffle furnace to form the perovskite phase.
The crystalline phase structures of both PNC73 powder and BCZYYb4411 powder were examined by X-ray diffraction (XRD, Rigaku SmartLab). Utilizing ESEM analysis (TFS Quattro S) in a secondary electron mode, the morphology of both the whole cell structure and the post-test cell structure was assessed, with a particular emphasis on the cross-sectional view.
| This journal is © The Royal Society of Chemistry 2024 |