aResearch Institute of Interdisciplinary Sciences (RISE) and School of Materials Science & Engineering, Dongguan University of Technology, Dongguan 523808, Guangdong, China
bDepartment of Physical and Macromolecular Chemistry, Faculty of Science, Charles University, Hlavova 8, Prague 2 128 43, Czech Republic. E-mail: mariya.shamzhy@natur.cuni.cz
cICGM, Univ Montpellier, CNRS, ENSCM, Montpellier, France. E-mail: anne.galarneau@enscm.fr
First published on 1st February 2024
Hierarchical zeolite catalysts containing additional meso- or macropores have attracted significant interest due to their beneficial performance in various reactions involving bulky molecules. A surfactant-templated post-synthesis of zeolites in basic medium (NaOH) advances from the uniform mesopore size distribution and easy regulation of micro-to-mesopore volume ratio in thus prepared hierarchical zeolites, although their synthesis–acidity–performance relationships remain elusive. In this study, we tackled this problem by designing a series of surfactant-templated hierarchical FAU catalysts with systematically varied textural and acidic characteristics, while assessing their catalytic performance in two model reactions: (1) acid-site-strength insensitive O-alkylation of bulky alcohols (1-octadecanol and 1-adamatylmethanol) and (2) acid-site-strength sensitive Friedel–Crafts benzoylation of p-xylene. A systematic increase in the NaOH/Si molar ratio in the synthesis from 0.075 to 0.25 decreased the number of strong Brønsted acid sites in hierarchical FAU zeolites, while it increased the concentration of Brønsted acid sites accessible for bulky molecules (up to 67% in hierarchical zeolites vs. 21% in the parent FAU zeolite). The development of transport mesopores was shown to positively affect the outcome of the studied reactions independently of the required acid site strength. Although, the optimal interplay between the concentration of strong Brønsted acid sites and their ‘accessibility’ (i.e., fraction of acid sites accessible to molecules with a kinetic diameter larger than the micropore opening in zeolites) was found to differ for O-alkylation of bulky alcohols or Friedel–Crafts benzoylation of p-xylene, the possibility of balancing these characteristics in the hierarchical surfactant-templated zeolites was shown by adjusting the NaOH/Si ratio used for their preparation. The results of this study contribute to the understanding of the synthesis–property–performance relationships of surfactant-templated hierarchical zeolite catalysts and provide a guide to tailor the best catalyst for a given reaction.
To eliminate diffusion restrictions and to enhance the catalytic activity of zeolites in the transformation of bulky molecules, many synthetic strategies have been developed for the preparation of zeolite catalysts with additional meso- or macroporosity.7 Traditionally, secondary porosities are introduced into zeolites by post-synthesis demetallation methods, including dealumination,8 desilication,9 degermination,10 and unbiased dealumination/desilication.11,12 The demetallation approach benefits from a simple and cheap synthesis protocol but produces hierarchical zeolites with mesopores, which are mostly embedded inside the crystals; as a result, the developed mesoporosity provides limited improvement in the transport of reacting molecules to/from the active sites of a catalyst. Hierarchically porous zeolites could also be generated by the addition of hard or soft templates as mesoporogens during direct hydrothermal synthesis.13–16 The obtained hierarchical zeolites have uniform transport mesopores, although using mesoporogens may hinder the formation of the targeted zeolite phase. In addition, there are several mesoporogen-free methods that are implemented using seed assistance17,18 and crystallization kinetic regulation,19–21 thus requiring careful optimization of the synthesis conditions. Hierarchical zeolites have been tested in various catalytic reactions, such as catalytic cracking of hydrocarbons,22 methanol to hydrocarbons,23 Fischer–Tropsch synthesis,24 Friedel–Crafts acylation25 and alkylation26,27 reactions among others, in which they showed remarkably improved catalytic activity, selectivity, or stability compared to traditional zeolites.
In addition to the above-mentioned preparation strategies, the surfactant-templating approach was developed for straightforward synthesis of hierarchical zeolites with uniform transport mesopores.28 This method combines (i) the partial dissolution of the initial zeolite in the basic medium (for example, an aqueous solution of NaOH) in the presence of alkyltrimethylammonium bromide containing 10–22 carbon atoms in the alkyl chain (CnTAB, n = 10–22), (ii) simultaneous rearrangement of the formed debris around the CnTAB micelles under hydrothermal conditions and (iii) the removal of surfactant from the formed zeolite–surfactant composite by calcination, which releases the voids with sizes resembling the diameter of micelle and corresponding to the formation of uniform mesopores. In this way, hierarchical zeolites of different types with a uniform size distribution of introduced mesopores were prepared. The advantage of the surfactant-assisted method is that the mesopore-to-micropore volume ratio of the produced zeolites could be varied by a simple adjustment of the basicity in the synthetic mixture. Using this method, Mehlhorn et al. synthesized a family of micro–mesoporous FAU zeolites in the presence of octadecyltrimethylammonium surfactant.29,30 These materials feature uniform mesopores of ca. 4 nm diameter, while their textural and acidic properties varied depending on the NaOH/Si ratio used in the reacting mixture. Similarly, Desmurs et al. obtained a series of surfactant-templating hierarchical MFI zeolites with variable mesopore volumes by tuning the NaOH/Si ratios in the synthesis gel.31 They observed that increasing the NaOH/Si ratio resulted in zeolites with a higher mesopore volume but a decreased Brønsted acid site concentration. Among the studied zeolite catalysts, the micro–mesoporous MFI zeolites obtained with NaOH/Si = 0.38 showed the highest yield in the synthesis of 2,4-di-tert-butylphenol through alkylation of phenol with tert-butyl alcohol, while the micro–mesoporous MFI catalyst prepared using NaOH/Si = 0.50 was the most active in the esterification of benzyl alcohol with hexanoic acid. The obtained results reflect a generally accepted increase in the activity of zeolite catalysts in the transformation or synthesis of bulky molecules with both the ‘accessibility’ and the number of acid sites,32,33 although, to our best knowledge, clear synthesis–acidity–performance relationships for surfactant-templating zeolites remain elusive. As both the reactants transport to/from active sites and the characteristics of active sites play an important role in the catalytic transformations over zeolite catalysts, understanding the effect of synthesis conditions on the characteristics of surfactant-templating hierarchical zeolites would open the way to rational optimization of their properties for a given catalytic reaction.
This work aimed at understanding the synthesis–property–performance relationships in surfactant-templating zeolites taking the FAU structural type as a representative example. For that, we have designed and synthesized a series of micro–mesoporous FAU zeolites with systematically varied micropore-to-mesopore volume ratios, comprehensively characterized the textural and acidic properties of the as-prepared catalysts using various techniques (e.g., transmission electron microscopy, X-ray diffraction, nitrogen physisorption, FTIR spectroscopy of adsorbed probe molecules) and related them to the catalytic performance of the designed zeolites in tetrahydropyranylation of bulky alcohols and acylation of p-xylene, representing acid-site-strength insensitive and acid-site-strength sensitive reactions, respectively. The obtained results are expected to further the understanding of synthesis–property–performance relationships of surfactant-templated hierarchical zeolite catalysts and to provide a guide for optimizing their properties for a given catalytic reaction.
Powder X-ray diffraction (XRD) patterns of the catalysts were collected using a Bruker D8 Advance diffractometer using Cu Kα radiation (30 kV, 40 mA). The textual properties of the catalysts were determined by nitrogen sorption isotherms at −196 °C using an ASAP 2020 Micromeritics apparatus. 100 mg of materials were outgassed under vacuum at 350 °C for 6 h prior to nitrogen sorption analysis. The specific surface area was determined using the BET method. The relative pressure range to use the BET equation (p/p0)/[V(1 − p/p0)] = f(p/p0) was determined using the superior limit given by the maximum of the Rouquerol curve V(1 − p/p0) = f(p/p0).35 The mesopore pore-size distribution was evaluated using the Broekhoff and de Boer (BdB) method36 at the inflection point of the desorption step, while the values of micropore and mesopore volumes and surfaces were determined by the corrected t-plot method.30,37 As a comparison and to establish pore size distribution for micro- and mesopores, pore diameters were also calculated by the NLDFT method with software SAIEUS of Micromeritics (model: zeolites (H-form)-N2-77, NLDFT (cylindrical)) using the desorption branch of the isotherms.
Concentrations of Lewis (CLAS) and Brønsted (CBAS) acid sites were determined after adsorption of pyridine (Py) by Fourier-transform infrared spectroscopy (FTIR) on Nicolet iS50 FTIR with MCT/B detector. The zeolites were pressed into self-supporting wafers with a density of 8–12 mg cm−2 and activated in situ at 450 °C for 4 h. Pyridine adsorption was carried out at 150 °C for 20 minutes at 600–800 Pa partial pressure, followed by desorption for 20 minutes at 150, 250, 350 or 450 °C. Before adsorption, pyridine was degassed by freezing and thawing cycles. All spectra were recorded with a resolution of 4 cm−1 by collecting 128 scans for a single spectrum at room temperature. Spectra were calculated at a wafer density of 10 mg cm−2. The total concentration of BAS (CBAS-Py) and LAS (CLAS-Py) was evaluated from the integral intensities of the absorption bands at 1545 cm−1 1455 cm−1 after pyridine desorption at 150 °C using molar absorption coefficients, ε1545 = 1.54 cm μmol−1, and ε1545 = 1.71 cm μmol−138 according to the following equations:
(1) |
(2) |
To estimate the fraction of strong Lewis and Brønsted acid sites, the intensity of the characteristic bands at 450 °C was related to those at 150 °C as follows:
(3) |
(4) |
A relatively large probe molecule 2,6-di-tert-butylpyridine (DTBP) with a kinetic diameter of 0.79 nm40 was used to determine the ‘accessibility’ of acid sites within prepared zeolites.41 DTBP adsorption took place at 150 °C at equilibrium probe vapour pressure for 15 minutes. Desorption proceeded at the same temperature for 1 hour, followed by the collection of spectra at room temperature. Molar absorption coefficient from ref. 42 was used for the evaluation of CBAS accessible for DTBP using the integral intensity of the absorption band at ca. 3360 cm−1.
The liquid-phase acylation reaction was performed at 130 °C. p-Xylene (5 mL), internal standard (dodecane, 0.25 g), and the catalyst (50 mg) were added to a three-neck flask. Benzoyl chloride (5 mmol) was added to the flask when the required temperature was reached.
The samples of the reaction mixture were taken periodically and analyzed using a gas chromatography instrument (Agilent 7890B) equipped with a HP-5 column (30 m × 0.32 mm × 0.25 μm) and an FID detector.
Conversion (X), yield (Y) and selectivity (S) were calculated according to the following equations:
X = [(n(reactant)0 − n(reactant)t)/n(reactant)0] × 100[%] | (5) |
Y = [n(product)t/n(reactant)0] × 100[%] | (6) |
S = [Y/X] × 100[%] | (7) |
The activity of zeolite catalyst was assessed by their initial reaction rate per acid site. The initial reaction rate was calculated as a slope to the graph of product concentration against the reaction time at t = 0 and then normalized to the total concentration of BAS and LAS as determined by FTIR-Py after desorption of the probe molecule at 150 °C (Rtotal) or to the concentration of strong BAS and LAS as determined by FTIR-Py after desorption of the probe molecule at 450 °C (Rstrong).
In agreement with the TEM results, the XRD patterns of the initial CBV720 and NaOH/Si-n (n = 0.075; 0.095; 0.125) samples clearly show intensive Bragg peaks characteristic of FAU zeolite (e.g., 111, 220, 311, 331 in Fig. 2a), while NaOH/Si-0.25 demonstrated a remarkable decrease in the intensity of these diffraction lines.46 In particular, the intensities of the peaks attributed to FAU zeolite decreased in the following order CBV720 > NaOH/Si-0.075 ≈ NaOH/Si-0.095 > NaOH/Si-0.125 ≫ NaOH/Si-0.25, which suggested a higher depletion of zeolite phase for the samples synthesized at higher NaOH/Si. Another characteristic feature seen in XRD patterns of NaOH/Si-n samples is the appearance of the low-angle 2θ peak at around 2° (Fig. 2b), indicating the mesoscale ordering.47
Fig. 2 Powder XRD patterns (a) and (b), N2 sorption isotherms at 77 K (c) and NLDFT pore size distribution (d) of FAU-Y (CBV720) and micro–mesoporous FAU zeolites (NaOH/Si-n). |
The nitrogen sorption isotherms of NaOH/Si-n zeolites exhibit a combined type I + IV, characteristic of materials possessing both micro- and mesopores (Fig. 2c). A steep increase in the adsorbed amount in the range of 0.35 < p/p0 < 0.55 characteristic of all NaOH/Si-n materials suggested a narrow mesopore size distribution29 centered at 4.0–4.5 nm (as evaluated by the BdB and NLDFT methods, Table 1). Both mesopore-to-micropore volume ratios and surface areas of hierarchical surfactant-templated NaOH/Si-n zeolites increased as the n value grew (Table 1). Notably, all NaOH/Si-n samples with n < 0.25 possess a similar external surface area (50 m2 g−1) and high CBET parameters (578–815) as expected for materials containing micropores. On the contrary, NaOH/Si-0.25 has a larger external surface area (90 m2 g−1) (Table 1), but CBET as low as 125. The results of physisorption validate NaOH/Si-0.25 as close to a pure mesoporous catalyst, similar to the Al-MCM-41-type material, although containing some strong Brønsted acid sites (vide infra).
Catalyst | Relative pressure regiona | S BET (m2 g−1) | C BET | S mic (m2 g−1) | S mes (m2 g−1) | S ext (m2 g−1) | V tot (mL g−1) | V mic (mL g−1) | V mes (mL g−1) | D BdB (nm) | D NLDFT (nm) |
---|---|---|---|---|---|---|---|---|---|---|---|
a Relative pressure domain for SBET calculation obtained following Rouquerol criteria.37 b Determined by the corrected t-plot method.37 c V mic supercage = 0.28 mL g−1; supercages could remain in these FAU zeolites. d Some mesopores are present in the initial dealuminated FAU-Y (CBV720), as observed by TEM, but they are mainly embedded inside the crystals without connections to the exterior of the crystals, as revealed by the horizontal hysteresis characteristic of cavitation phenomenon in the nitrogen sorption isotherm. However, a small fraction of mesopores is connected to the exterior of the crystals, as observed by the vertical hysteresis at p/p0 ∼ 0.90, corresponding to mesopores of 22 nm diameter and a mesopore volume of ∼0.09 mL g−1. These very large mesopores are not counted in the corrected t-plot method, and the external surface area can be counted as the mesopore surface area for CBV720. e Pore diameters calculated by the NLDFT method with software SAIEUS of Micromeritics model: zeolites (H-form)-N2-77, NLDFT (cylindrical) are given for comparison. Micropore diameters calculated by this method were 0.63 nm for FAU-Y (CBV720), NaOH/Si-0.075 and NaOH/Si-0.095, and 0.61 nm for NaOH/Si-0.125 and NaOH/Si-0.25. FAU-Y features windows of 0.74 nm and cavities of 1.3 nm, and the chosen NLDFT model gives an equivalent cylindrical diameter of 0.63 nm. | |||||||||||
CBV720 | 0.001–0.043 | 946 | 2304 | 832 | 0d | 99 | 0.37 | 0.37c | 0d | 22d | 25 |
NaOH/Si-0.075 | 0.010–0.075 | 910 | 815 | 581 | 280 | 49 | 0.53 | 0.32c | 0.21 | 4.3 | 4.5 |
NaOH/Si-0.095 | 0.010–0.100 | 934 | 578 | 493 | 390 | 51 | 0.62 | 0.28c | 0.34 | 4.3 | 4.4 |
NaOH/Si-0.125 | 0.019–0.126 | 879 | 707 | 349 | 477 | 53 | 0.65 | 0.22 | 0.44 | 4.2 | 4.3 |
NaOH/Si-0.25 | 0.040–0.275 | 969 | 123 | 44 | 835 | 90 | 0.81 | 0.02 | 0.78 | 4.0 | 3.9 |
The type, concentration, and strength of acid sites in the designed hierarchical FAU zeolites were determined by FTIR spectroscopy using probe molecules of different kinetic diameters: pyridine (0.54 nm) and 2,6-di-tert-butylpyridine (0.79 nm). The spectra of activated CBV720 and NaOH/Si-n samples showed the bands corresponding to the Brønsted acid sites (BAS) in the OH vibration region (3631 and 3565 cm−1, Fig. 3a), while the adsorption of pyridine completely removed these bands, suggesting the 100% ‘accessibility’ of BAS in all the studied materials for the pyridine probe. Analysis of the characteristic absorption bands in the FTIR-Py spectra revealed a remarkable decrease in the concentration of BAS (by 35–68%) and less severe drop in the number of Lewis acid sites (by 11–21%) in micro–mesoporous NaOH/Si-n zeolites (n = 0.075; 0.095; 0.125) compared to the initial CBV720 (Fig. 3c and Table 2). Among NaOH/Si-n samples, the zeolite-poor mesostructured NaOH/Si-0.25 showed the highest drop in BAS concentration by 78%, but increased number of Lewis acid sites. Notably, zeolite-poor mesostructured NaOH/Si-0.25 possessed significantly lower part of strong BAS (Fig. 3b), while the micro–mesoporous FAU NaOH/Si-n samples (n = 0.075; 0.095; 0.125) prepared with lower NaOH/Si ratios contained a similar fraction of strong Brønsted and Lewis acid sites retaining pyridine at 450 °C as the initial CBV720 zeolite.
Catalyst | Pyridine (mmol g−1) | DTBP (mmol g−1) | ||
---|---|---|---|---|
C BAS-Py | C LAS-Py | LAS/BAS | C BAS-DTBP | |
a The values in brackets show the % change in the concentration of acid sites in NaOH/Si-n samples compared to the initial CBV-720. b The values in brackets are the ratio of CBAS-DTBP to CBAS-Py, indicating the % of BAS accessible for DTBP. | ||||
CBV720 | 0.37 | 0.19 | 0.5 | 0.08 (21%)b |
NaOH/Si-0.075 | 0.24 (−35%)a | 0.17 (−11%)a | 0.7 | 0.07 (29%)b |
NaOH/Si-0.095 | 0.18 (−51%)a | 0.15 (−21%)a | 0.8 | 0.08 (44%)b |
NaOH/Si-0.125 | 0.13 (−68%)a | 0.15 (−21%)a | 1.2 | 0.07 (54%)b |
NaOH/Si-0.25 | 0.09 (−76%)a | 0.21 (+11%)a | 2.3 | 0.06 (67%)b |
At the same time, compared to the initial CBV720 sample, the fraction of Brønsted acid sites accessible for DTBP increases greatly for NaOH/Si-n (n = 0.095; 0.125; 0.25) (44–67%, Table 2), while NaOH/Si-0.075 prepared with the lowest NaOH/Si ratio showed just a slight increase in BAS ‘accessibility’ compared to CBV720 (29%). This result is in line with a decrease in the size of the crystalline zeolite domains of the FAU samples confirmed by TEM (Fig. 1) and an XRD (Fig. 2) and increase in the fraction of mesopores confirmed by nitrogen physisorption (Table 1).
The decrease in BAS concentration appears to follow the decrease in the micropore surface area (Fig. 4) (and a related increase in the mesopore surface area). To understand the influence of the collaborative change in textural properties (facilitating the transport of reacting molecules) and acidic characteristics (decreasing the number of catalytically active sites) in surfactant-templating hierarchical zeolites on their catalytic performance, the designed series of NaOH/Si-n catalysts were tested in model reactions with different requirements to the strength of acid sites: (1) O-alkylation of alcohols which proceeds on both strong acid sites and acid centers of relatively low strength; and (2) Friedel–Crafts acylation, requiring relatively strong acid sites.
Similarly, in the O-alkylation of bulkier 1-adamantanemethanol, all surfactant-templated micro–mesoporous FAU zeolites outperformed the initial CBV720 (1-adamantanemethanol conversion after 360 min of 13–21% for NaOH/Si-n vs. 8% for initial FAU-Y, Fig. 5c). The highest conversion of 1-adamantanemethanol was observed over NaOH/Si-0.95 prepared at a medium NaOH/Si molar ratio. Compared to NaOH/Si-0.95, less active NaOH/Si-n showed a smaller mesopore volume (n = 0.075, Fig. 4) or a lower concentration of Brønsted acid sites (n = 0.125 and n = 0.25, Fig. 4).
Incomplete conversion of both alcohols even for the most active FAU NaOH/Si-n catalysts can be partially related to the reversible character of tetrahydropyranylation reaction53 and catalyst deactivation. The generally lower conversion reached for 1-adamantanemethanol compared to 1-octadecanol over the studied zeolite catalysts may be explained by the difference in the reactivity of two alcohols, including diffusion restrictions. While a rigid adamantyl alkyl substituent provides permanent bulkiness to the respective reactant molecule, the long-chain 1-octadecanol molecule can exist in a linear or elongated conformation. This conformational flexibility is assumed to increase the probability of transformation of 1-octadecanol at the active sites located at the micropore entrances in comparison to 1-adamantanemethanol, while the acid sites at the external surface are considered accessible for both alcohol reactants.
To provide more insight into the acidity–activity relationships for O-alkylation of bulky alcohols over surfactant-templated micro–mesoporous FAU zeolites, we further estimated the activity of the catalysts. Specifically, we estimated the catalysts’ activity in terms of initial reaction rates (R) normalized per acid site.54 This metric represents the number of reactant molecules converted per acid site per hour and was calculated based on the slope to the graph of products concentration against the reaction time at t = 0. This calculation was made under the assumption that catalyst deactivation at this initial point was negligible. In addition, although the initial reaction rate may vary depending on experimental conditions, such as the initial concentrations of reagents, it was considered a reliable descriptor of the studied catalysts as the catalytic experiments were conducted under identical conditions. Thus evaluated initial rate values were separately analyzed for acid sites that retain pyridine at 150 °C (Rtotal, Fig. 6a and b) and for the strongest acid sites that retain pyridine at 450 °C (Rstrong, Fig. 6c and d). These activity indicators enable a direct comparison of catalysts containing different concentrations of acid sites and differing in their strength.
For both 1-octadecanol and 1-adamantanemethanol, Rtotal values increased in the order of CBV720 < NaOH/Si-0.075 < NaOH/Si-0.095 < NaOH/Si-0.25 < NaOH/Si-0.125 (Fig. 5a and c). Except for NaOH/Si-0.25 (showing a markedly lower fraction of strong acid sites compared to other catalysts studied), the increase in catalyst activity corresponds to the increase in the volume of transport mesopores (Fig. 4). In turn, the obtained Rstrong values suggest a similar intrinsic activity of acid sites with similar strength to NaOH/Si-0.125 and NaOH/Si-0.25 with the highest ‘accessibility’ of acid centers showing similar Rstrong (Fig. 5b and d).
A comparison of NaOH/Si-n and CBV720 catalysts in the acid-site-strength insensitive tetrahydropyrahylation of 1-octadecanol and 1-adamantanemethanol revealed a positive effect of the development of transport mesopores in hierarchical surfactant-templated FAU zeolites for either conformationally flexible or rigid bulky alcohols, the trend, which is not compromised by either increase in LAS/BAS ratio or decrease in the total concentration of acid sites.
Over FAU-Y (CBV720) and micro–mesoporous FAU zeolites (NaOH/Si-n) catalysts, 2,5-dimethylbenzophenone was formed as the main product (selectivity > 80%). The formation of the undesired benzoic anhydride product increased with decreasing concentration of strong acid sites according to previous reports.55,56 At 15% benzoyl chloride conversion, the selectivity in the undesired benzoic anhydride product increased in the following order: NaOH/Si-0.075 (1%) < NaOH/Si-0.095 (5%) < NaOH/Si-0.125 (7%) < NaOH/Si-0.25 (20%). Among hierarchical FAU zeolites, only NaOH/Si-0.075 with the highest fraction of the remaining zeolite phase and the highest concentration of Brønsted acid sites outperformed the initial CBV720 in terms of benzoyl chloride conversion (Fig. 7b) and yield of 2,5-dimethylbenzophenone (Fig. 8).
NaOH/Si-n (n = 0.095, 0.0125 and 0.25) catalysts with lower concentration of BAS and higher LAS/BAS ratio showed lower yields of 2,5-dimethylbenzophenone in comparison to the initial CBV720 zeolite (Fig. 8). As mentioned above, the acylation reaction is generally promoted by medium and strong acid sites on zeolite catalysts, while the probability of “product inhibition” increases with the LAS/BAS ratio.55,57 Therefore, the enhanced benzoyl chloride conversion and target product selectivity over NaOH/Si-0.075 should be attributed to the higher concentration of strong acid sites, lower LAS/BAS ratio in this hierarchical zeolite in comparison to NaOH/Si-n (n = 0.095, 0.0125 and 0.25) and better transport of reagents compared to CBV720. Rtotal numbers calculated based on the total concentration of Brønsted and Lewis acid sites in hierarchical zeolites showed an interesting trend, suggesting the importance of the acid site type, rather than their ‘accessibility’ for the activity of a catalyst in the benzoylation of p-xylene. Specifically, after a notable increase in the Rtotal value for NaOH/Si-0.075 vs. initial CBV720, the Rtotal decreased in NaOH/Si-0.95 and was similar to NaOH/Si-n (n = 0.125; 0.25) despite an increase in the ‘accessibility’ of acid sites (Fig. 7c).
A comparison of NaOH/Si-n and CBV720 catalysts in Friedel–Crafts acylation of p-xylene with benzoyl chloride revealed that the best hierarchical zeolite catalyst for this reaction maintains a high concentration of BAS together with the addition of mesopores, which is in line with the crucial role of acid site type and strength for the Friedel–Crafts acylation reaction.
A systematic increase in the NaOH/Si ratio from 0.075 to 0.25 used for the surfactant-templating synthesis of hierarchical FAU zeolites led to a progressive decrease in the size of crystalline FAU zeolite domains resulting in: (1) an increase in the mesopore volume from 0.21 to 0.78 mL g−1; (2) a decrease in the micropore volume from 0.32 to 0.02 mL g−1; (3) an increase in the fraction of Brønsted acid sites accessible for 2,6-di-tert-butylpyridine from 29% to 67%; but (4) a decrease in the concentration of Brønsted acid sites characteristic of a zeolite phase.
A comparison of NaOH/Si-n and CBV720 catalysts in Friedel–Crafts acylation of p-xylene with benzoyl chloride and in the tetrahydropyrahylation of 1-octadecanol and 1-adamantanemethanol suggests that the development of transport mesopores in hierarchical surfactant-templated FAU zeolites positively affected their performance in either acid-site-strength sensitive and acid-site-strength insensitive reactions. However, the optimised micro–mesoporous zeolite catalysts are different for the reactions studied (Fig. 8). For the O-alkylation reaction, which requires moderate acidity, hierarchical zeolites prepared in a NaOH/Si ratio of 0.095 or 0.125 and featuring highly developed mesoporosity (e.g., mesopore volume >0.33 mL g−1) were the most active catalysts, despite a drop in the concentration of strong BAS. In turn, for catalytic reactions that need strong acid sites, such as acylation, the best catalyst was NaOH/Si-0.075, which maintains a high concentration of BAS (0.24 mmol g−1) together with the addition of mesopores (0.21 mL g−1). The results obtained in this work complete our understanding of synthesis–property–performance relationships of zeolite catalysts and open the way to rational fine-tuning of their properties.
This journal is © The Royal Society of Chemistry 2024 |