Facile fabrication of CoAl-LDH nanosheets for efficient rhodamine B degradation via peroxymonosulfate activation

Hui Fui*, Shumin Gao, Xinran Ma and Yiping Huang
School of Chemical and Environmental Engineering, Wuhan Polytechnic University, Wuhan 430023, Hubei Province, PR China. E-mail: feihui509@163.com

Received 9th July 2023 , Accepted 27th September 2023

First published on 10th October 2023


Abstract

Layered double hydroxides (LDHs) have been extensively investigated as promising peroxymonosulfate (PMS) activators for the degradation of organic pollutants. However, bulk LDHs synthesized using conventional methods possess a closely stacked layered structure, which seriously blocks active sites and yields low intrinsic activity. In this study, we exfoliated bulk CoAl-LDHs to fabricate CoAl-LDH nanosheets by alkali-etching and Ostwald ripening via a simple hydrothermal process in a KOH solution. The exfoliated LDHs possessed the typical nanosheet structure with more exposed active sites for PMS activation, and hence, boosted the degradation of the pollutants. CoAl-1 exhibited an outstanding catalytic performance as the PMS activator for rhodamine B (RhB) degradation with the apparent rate constant of 0.1687 min−1, which was about 3.63 and 5.02 times higher than that of commercial nano-Co3O4 and bulk CoAl-LDH, respectively. The maximum RhB degradation of 93.1% was achieved at the optimal reaction conditions: catalyst dose 0.1 g L−1, PMS concentration 0.3 mM, pH 7, and temperature 298 K. Further analysis of RhB degradation mechanism illustrated that singlet oxygen (1O2) dominated RhB degradation in the CoAl-1/PMS system, while ˙OH, ˙O2, and ˙SO4 may mainly serve as the intermediates for the generation of 1O2 and were indirectly involved in the degradation. This study provides a promising strategy for developing two-dimensional LDH nanosheets for wastewater remediation.


1. Introduction

The intensification of organic pollutants, such as pesticides, pharmaceuticals, personal care products, and organic dyes, in water seriously threatens human health and has acquired tremendous attention.1–5 Numerous technologies (e.g., adsorption method, membrane separation, bio-degradation, and advanced oxidation processes (AOPs)) have been undertaken to eliminate these organic pollutants from water.6–9 Among them, persulfate-based advanced oxidation processes have been recognized as a highly promising approach where the activation of persulfates (peroxymonosulfate (PMS) and peroxydisulfate (PDS)) can produce a series of powerful species (e.g., ˙SO4, ˙OH, and 1O2), and these species can degrade or mineralize organic contaminants.10 In general, PMS can be more easily activated than PDS in homogeneous or heterogeneous systems by means of various methods (e.g., thermal, ultraviolet, alkaline, transition metals, and carbon materials).11–15 However, transition metals (e.g., Co, Mn, and Cr) are a feasible way to activate PMS.16,17 Unfortunately, transition metal ions used in the homogeneous system are difficult to recover from the reaction solution and inevitably cause secondary pollution. Thus, the construction of high-performance heterogeneous catalysts as PMS activators is highly desired.

As typical transition metal-based materials, layered double hydroxides (LDHs) with positively charged host layers and intercalated charge balancing anions18–20 are regarded as promising PMS activators for organic pollutant degradation because of their highly controllable layered structure and metal composition (e.g., interlayer anions, number of layers, metal species, and metal ratios).21–23 However, LDH layers tend to stack or even form bulk LDHs with the closely stacked layered structure, which blocks active sites and leads to low catalytic activities.24 In this regard, the exfoliation of bulk LDHs into LDH nanosheets is an effective strategy to increase the surface area and exposed active sites. Thus, numerous strategies have been developed to exfoliate the pristine bulk LDH into ultrathin nanosheets. Zhang et al.25 reported a two-step strategy to exfoliate bulk LDHs using zwitterionic surfactants, in which zwitterionic surfactants were first inserted into the LDH interlayers by ion exchange, and then the surfactant-intercalated LDHs were exfoliated to obtain LDH nanosheets in an organic solvent. Yu et al.26 prepared LDH nanosheets by exfoliating bulk LDHs directly in a formamide solution without the pre-synthesis of surfactant-intercalated LDHs. Nevertheless, organic solvents used in the above exfoliation process tend to attach on the surface of the obtained LDH nanosheets, thus blocking the exposed active sites.27,28 Recently, Chen et al.29 presented a novel exfoliation method for NiFe LDHs by Ostwald ripening via a simple hydrothermal treatment without using extra reagents or surfactants. Nevertheless, the Ostwald ripening driven exfoliation usually takes a long time. Therefore, an efficient strategy needs to be explored for fabricating clean LDH nanosheets by exfoliating the bulk LDHs.

Herein, we report an exfoliation strategy of bulk CoAl-LDHs to afford two-dimensional nanosheets by alkali-etching and Ostwald ripening via a facile hydrothermal treatment in KOH solution. The best samples exhibited superior catalytic activity for RhB degradation compared with bulk CoAl-LDHs and commercial nano-Co3O4. Moreover, the effect of the reaction parameters (e.g., pH, temperature, catalyst dosage, and PMS concentration) on RhB degradation was systematically investigated. Further analysis of the RhB degradation mechanism in the CoAl-1/PMS system was performed using electron paramagnetic resonance (EPR) and a series of scavenger experiments. This study provides a promising strategy for developing thin-layer LDHs for the removal of organic pollutants.

2. Experimental section

2.1 Materials and reagents

Cobaltous nitrate hexahydrate (Co(NO3)2·6H2O), sulfuric acid (H2SO4), sodium carbonate (Na2CO3), aluminum nitrate nonahydrate (Al(NO3)3·9H2O), sodium thiosulfate (Na2S2O3), furfuryl alcohol (FFA), 5,5-dimethyl-1-pyrroline N-oxide (DMPO), rhodamine B (RhB), potassium peroxymonosulfate (PMS), tert-butyl alcohol (TBA), 2,2,6,6-tetramethyl-4-piperidone (TMP), p-benzoquinone (p-BQ), methanol (MeOH), and commercial nano-Co3O4 (30 nm, 99.5%) were supplied by Aladdin Company, China and used as received. Deionized water was used in all the experiments.

2.2 Catalyst preparation

CoAl-LDHs were synthesized using a conventional coprecipitation method. Typically, solution A was pre-prepared by adding Co(NO3)2·6H2O (0.08 mol), Al(NO3)3·9H2O (0.04 mol) to deionized water (80 mL). Then, 80 mL of solution B containing NaOH (0.24 mol) and Na2CO3 (0.2 mol) was added dropwise to solution A under magnetic stirring. After continuously stirring for 0.5 h, the resulting suspensions were aged at 60 °C for 24 h in a water bath. Finally, the precipitate was washed several times with deionized water and ethanol and then dried at 60 °C overnight in a vacuum to obtain CoAl-LDHs.

CoAl-LDH nanosheets were synthesized by exfoliating the CoAl-LDHs precursor through a simple hydrothermal treatment in KOH aqueous solution. Briefly, 300 mg CoAl-LDHs was added to a 100 mL Teflon-lined autoclave with 80 mL of potassium hydroxide aqueous solution (0.5 M). The autoclave was then heated to 120 °C and maintained for different times. Afterward, the resulting product was rinsed with deionized water and ethanol several times and dried at 60 °C under vacuum for 24 h to obtain exfoliated CoAl-LDH. According to different hydrothermal times (0.5, 1, and 2 h), the as-prepared exfoliated CoAl-LDH samples were labeled as CoAl-0.5, CoAl-1, and CoAl-2, respectively. For comparison, the samples (denoted as CoAl-W) were fabricated under the same hydrothermal conditions for 1 h without the addition of KOH.

2.3 Catalyst characterization

The phase structures of the as-fabricated catalyst were analyzed by X-ray powder diffraction (XRD) on a Bruker D8 Advance powder diffractometer using Cu Kα radiation (λ = 0.154 nm). The morphology was examined using a Zeiss GeminiSEM 300 scanning electron microscope (SEM). Elemental mappings were performed by energy-dispersive X-ray spectroscopy (EDS, Oxford X-MAX) on the SEM tool. X-ray photoelectron spectroscopy (XPS) was conducted on a Thermo Scientific Escalab 250Xi spectrometer with an Al Kα anode, and the binding energy was standardized with respect to the residual C 1s peak.

2.4 Experimental procedures

PMS activation performance of the as-fabricated catalyst was evaluated using RhB as a probing molecule. Typically, 10 mg catalyst was added to 100 mL of RhB solution (80 mg L−1) under mechanical stirring. Afterward, 0.3 mM PMS was added to the suspension to initiate the reaction. 2 mL samples were withdrawn at regular intervals, quenched with Na2S2O3 solution, and filtered using a 0.22 μm filter. The concentrations of RhB were analyzed using a UV-vis spectrophotometer (Lambda 650). 0.1 M NaOH or 0.1 M H2SO4 was used to adjust the initial pH values. To explore the mechanism of RhB degradation, electron paramagnetic resonance (EPR) was performed on a Bruker A300 spectrometer to identify the presence of reactive species. A series of quenching experiments were conducted using TBA, FFA, methanol, and p-BQ as radical scavengers to investigate the effect of these species on RhB degradation.

3. Results and discussion

3.1 Synthesis and characterization of catalysts

As illustrated in Fig. 1, the synthesis of CoAl-LDH nanosheets involved the pre-synthesis of the CoAl-LDH precursor, followed by exfoliation of the as-prepared precursor. The morphology of bulk CoAl-LDH and the typical exfoliated samples (CoAl-1) were characterized by SEM. As shown in Fig. 2a and b, the bulk CoAl-LDH exhibited an agglomerated plate morphology with a lateral size of 8.0–10.0 μm and an average thickness of 5.0–7.0 μm, which indicated that the pristine bulk LDHs comprised of multitudinous closely stacked LDH layers. After the exfoliation process, the morphology of CoAl-1 was significantly different from that of bulk CoAl-LDHs. As shown in Fig. 2c and d, CoAl-1 displayed hexagonal nanosheet morphology. The average thickness decreased to about 7.5 nm, and the number of stacked layers also decreased to about 9 or 10 layers (since a single LDH layer has a thickness of about 0.8 nm (ref. 30)). Meanwhile, EDS mapping analyses (Fig. 2e) confirmed a homogeneous distribution of Co, Al, O, and C on the near surface of CoAl-1. Furthermore, the Co/Al molar ratio (2.1[thin space (1/6-em)]:[thin space (1/6-em)]1.0) in CoAl-1 was higher than that in the synthesis mixture (2.0[thin space (1/6-em)]:[thin space (1/6-em)]1.0), indicating that Al vacancies were introduced by the exfoliation of bulk LDHs. The study on the exfoliation of other bulk materials also showed similar results.31
image file: d3ra04575g-f1.tif
Fig. 1 Schematic illustration of the synthetic route of CoAl-LDH nanosheets. (Al/Co atomic ratio used in the coprecipitation was 1[thin space (1/6-em)]:[thin space (1/6-em)]2, hydrothermal temperature was 180 °C, and KOH concentration was 0.5 M).

image file: d3ra04575g-f2.tif
Fig. 2 Low and high magnification SEM images of CoAl-LDH (a and b) and CoAl-1 (c and d); EDS mapping images (e) of CoAl-1.

The crystal structures of bulk CoAl-LDH and the exfoliated CoAl-LDH were studied by XRD. As shown in Fig. 3a, each sample manifested the characteristic diffraction peak of a rhombohedral LDH structure,32 in which the peaks at 11.66, 23.57, 34.94, 39.42, 60.32, 60.72° were assigned to the (003), (006), (012), (015), (110) and (0015) crystal planes, respectively, of CoAl-LDH (PDF51-0045).33 Note that the diffraction peaks at 19.30°, and 20.53° could be indexed to Co-LDH (PDF30-0443) and CoOOH (PDF07-0169), respectively. This phenomenon could be attributed to the fact that these products could be generated and their crystal structures were well preserved during the fabrication of CoAl-LDHs. After the exfoliating process, the (003) peak (Fig. 3b) for exfoliated CoAl-LDHs material was located at lower 2θ angles compared with the corresponding reflection for bulk CoAl-LDH, which might be attributed to smaller crystal size and a higher degree of disorder, thereby, lowering the 2θ angle of the (003) reflection.34 Furthermore, the (110) peak (Fig. 3b) shifted to higher 2θ angles as the exfoliation time increased, suggesting an in-plane compressive strain was introduced in the LDH nanosheets. The compressive strain was mainly due to the loss of aluminum and oxygen ions from the host layers during the exfoliation process. Overall, the above results proved that CoAl-LDH nanosheets were successfully prepared by exfoliating bulk LDH via hydrothermal treatment in a KOH solution.


image file: d3ra04575g-f3.tif
Fig. 3 (a) XRD patterns of different samples; (b) 2-theta angle for the (003) and (110) peak.

The surface chemical bonding states of CoAl-LDHs and CoAl-1 were characterized by XPS measurements. The survey spectrum in Fig. 4a again confirms the presence of Co, Al, O, and C. In the Al 2p spectra (Fig. 4b), the main peak was corresponding to Al3+ species. However, the peak intensity of CoAl-1 decreased, and the peak positions shifted negatively compared with that of CoAl LDHs, which might be attributed to the introduction of Al vacancies during the exfoliation process, thus creating different chemical/electron environments for Al atoms. It was noted that Co 2p XPS spectra and O 1s spectra showed little difference in peak shapes and positions for the two samples. In the Co 2p spectra (Fig. 4c), the two peaks corresponding to Co 2p3/2 and 2p1/2, are centered at 781.1 and 797.0 eV, respectively. The Co 2p3/2 peak can be fitted by Lorentzian–Gaussian, and the three fitted peaks corresponding to Co2+, Co3+, and satellite peaks were located at 782.4, 780.5, and 802.1 eV, respectively.35 However, the Co2+/Co3+ molar ratio in CoAl-1 was calculated to be 0.524 from their fitted peak area ratio, which is higher than that (0.476) of CoAl-LDHs, implying partial Co3+ was reduced to Co2+ after the exfoliation process.


image file: d3ra04575g-f4.tif
Fig. 4 XPS spectra of different samples. (a) Survey; (b) Al 1s; (c) Co 2p; (d) O 1s.

As shown in Fig. 4d, the O 1s spectra were fitted into three peaks, which were located at 529.1, 530.6, and 532.1 eV, representing lattice oxygen (O2−), absorbed oxygen (O22− and O2), and hydroxyl groups (OH), respectively. The peak area of the adsorbed oxygen represents the oxygen vacancy content. According to their fitted peak area ratio, the oxygen vacancy content was estimated to be 40.3% for CoAl-1 and 40.2% for CoAl-LDHs. According to the XPS spectrum analysis, a more plausible explanation is that Al vacancies might introduce oxygen vacancies into the LDH during the exfoliation process, and subsequently, the localized electrons in the oxygen vacancies would lead to the reduction of Co3+ to Co2+. More Co2+ and oxygen vacancies were the excellent active sites for the activation of PMS and hence improved the degradation of the pollutant.

3.2 Catalytic performance evaluation

The catalytic activities of the as-synthesized catalysts were investigated by activating PMS for RhB degradation. As shown in Fig. 5a, only a very small amount of RhB was removed when PMS or each catalyst was presented separately, suggesting that neither the single chemical oxidation nor the adsorption process could efficiently remove RhB. However, RhB degradation efficiency was significantly enhanced to 76.6% within 15 min when CoAl-0.5 and PMS were simultaneously introduced into the system. The exfoliated CoAl-LDH prepared with different exfoliation times exhibited different catalytic activities for RhB degradation. The highest RhB removal efficiency (93.1%) was achieved when CoAl-1 was used as the PMS activator. However, further enhancement was not observed, instead a slight decrease in removal rate occurred in the CoAl-3/PMS system. Combining the results of the XRD analyses, we have demonstrated that the activity order of the exfoliated CoAl-LDH was similar to the 2θ angle of the (003) reflection, implying that the different catalytic performances of the three catalysts might be ascribed to the crystal size.
image file: d3ra04575g-f5.tif
Fig. 5 (a) Degradation kinetics and (b) rate constant of RhB for the exfoliated CoAl-LDH; (c) degradation kinetics and (d) rate constant of RhB for bulk CoAl-LDH and CoAl-1. Experiment conditions: pH = 7, T = 298 K, [RhB] = 80 mg L−1, [catalyst] = 100 mg L−1, [PMS] = 0.3. mM.

Fig. 5b shows the catalytic activities of bulk CoAl-LDH and CoAl-1. CoAl-1 had excellent RhB degradation efficiency (93.1%) within 15 min, which was almost 2.7 times higher than that of bulk CoAl-LDH (34.2%). For further comparison, we evaluated the catalytic degradation of RhB with CoAl-W and nano-Co3O4 under the same reaction conditions, and RhB removal was only 64.2% for CoAl-W, and 48.2% for nano-Co3O4. In addition, based on the pseudo-first-order kinetics model,36 the degradation rate constant (k) in different systems was calculated. As shown in Fig. 3b, the rate constant (k) of the CoAl-1/PMS system was about 0.1687 min−1, which was about 2.22, 3.63, and 5.02 times higher than that of CoAl-W, nano-Co3O4 and bulk CoAl-LDH, respectively. These results indicated the obvious superiority of CoAl-1 during the catalytic oxidation over those of the other catalysts under the same reaction conditions, which could be attributed to the fact that CoAl-1 possessed the typical 2-dimensional structure. As has been previously reported,37 RhB is mainly degraded via PMS activation on the surface of the catalyst. PMS activation starts with the adsorption of PMS on the catalyst surface. Next, the charge transfer between catalysts and PMS generates SO4˙, which ultimately leads to the degradation of organic pollutants. As a result, the typical 2-dimensional structure of CoAl-1 provides a large specific surface area and more exposed active sites, which facilitates the contact of the catalysts with PMS and organic pollutant molecules, thus further enhancing the adsorption and catalytic performance.

3.3 Effects of the reaction parameters on RhB degradation

Some key reaction parameters (e.g., initial solution pH, reaction temperature, catalyst dosage, and PMS concentration) of the CoAl-1/PMS system were investigated and optimized. As shown in Fig. 6a and b, the degradation efficiency of RhB was significantly increased from 26.9% to 93.1% within 15 min when the catalyst dosage was increased from 0.05 to 0.1 g L−1, and the corresponding degradation rate constants (k) was obviously increased from 0.01397 to 0.1687. It could be attributed to the fact that increasing the catalyst dosage resulted in more active sites for PMS activation and generated more powerful radical species, thus accelerating RhB degradation. Nevertheless, when the catalyst dosage was further increased from 0.1 to 0.2 g L−1, the improved RhB degradation was not observed. This phenomenon could be attributed to the fact that the free radicals were generated to a maximum degree from the fixed PMS. In addition, an overabundance of the catalyst would generate excess radicals, and the scavenging effect of the excessive radical species would also suppress the catalytic degradation of RhB.38 Therefore, the catalyst dosage of 0.1 g L−1 was selected as the proper dosage.
image file: d3ra04575g-f6.tif
Fig. 6 Effects of (a) catalyst dose, (c) PMS concentration, (e) initial solution pH, (f) solution temperature on RhB degradation efficiencies in CoAl-1/PMS system, and the corresponding fitting kinetic parameters of (b) catalyst dose and (d) PMS concentration. [Reaction conditions: [RhB] = 80 mg L−1, [PMS] = 0.3 mM, [catalyst] = 100 mg L−1, T = 298 K and pH = 7.]

As shown in Fig. 6c and d, the PMS concentration had a positive but limited effect on RhB degradation. The RhB degradation efficiency was gradually increased from 84.3% to 93.1% within 15 min when the PMS concentration was increased from 0.15 to 0.3 mM. Nevertheless, the RhB degradation efficiency only exhibited a negligible increase from 93.1% to 95.3% within 15 min when the PMS dosage was further increased from 0.3 to 0.6 mM. This phenomenon could be explained as follows. When the PMS concentration was insufficient, increasing the PMS concentration would accelerate PMS activation on the catalyst surface and produce more reactive species, thus leading to rapid RhB degradation. However, when PMS exceeded the optimal dose, excessive free radicals would be generated and then react with the excessive PMS or undergo self-quenching reactions, producing some weaker oxidants and ultimately deteriorating RhB degradation. A similar study was performed by Li et al.39 on the degradation of MNZ, where they also found that the excessive PMS brought no obvious enhancement to MNZ degradation. Thus, the PMS concentration of 0.3 mM was selected as the optimal concentration.

As shown in Fig. 6e, RhB can be effectively decomposed in the pH range from 3–11 with a degradation efficiency of approximately 80% within 15 min, demonstrating that CoAl-1 could be used as an effective PMS activator for organic degradation over a wide pH range. Among them, increasing the initial pH from 3.0 to 7.0 accelerated RhB degradation efficiency from 85% to 93%. While RhB degradation efficiency instead declined from 93% to 79% with a further increase in pH from 7.0 to 11.0. The greatest removal efficiency (93.7%) was obtained at pH 7.0. This phenomenon could be explained as follows: the pKa1 and pKa2 of PMS were less than 0 and 9.4, respectively,40,41 and the pHzpc of the CoAl-1 catalyst was 6.8. According to the pHzpc, the catalysts possessed a positively charged surface under acidic conditions, while the catalysts possessed a negatively charged surface under alkaline conditions. As a result, when the initial pH was increased from 3.0 to 7.0, more HSO5 would be generated from PMS and was brought closer to the positively charged surface of the catalyst by the electrostatic gravitational forces, facilitating PMS activation thus yielding a faster RhB degradation. However, increasing the pH from 7.0 to 11.0 would enhance the electrostatic repulsion between the catalyst surface and PMS, constraining PMS activation on the catalyst surface, thus leading to lower RhB degradation. Besides, more sulfate radicals will be produced under acidic conditions, and conversely hydroxyl radicals will predominant alkaline conditions.42 When pH was increased from 7.0 to 11.0, the dominant species were hydroxyl radicals which were much weaker than sulfate radicals, leading to a lower degradation rate. Thus, the optimum pH for this process was 7.0.

As shown in Fig. 6f, the reaction temperature had a positive effect on RhB degradation. 93.1% of RhB was removed within 15 min at 25 °C. While 100% RhB could be degraded in 8, 6, and 4 min at 308, 318, and 328 K, respectively. The results indicated that higher temperatures could facilitate PMS activation to produce more ROS, thus accelerating RhB decomposition. RhB degradation kinetics were fitted to the pseudo-first-order kinetic model and the apparent rate constants (kobs) at 298, 308, 318, and 328 K were calculated to be 0.1687, 0.4142, 0.6279 and 0.9780 min−1, respectively. Based on the Arrhenius formula, the activation energy (Ea) in the CoAl-1/PMS system was calculated to be 42.23 kJ mol−1. The Ea value was much lower than that of ordinary reactions (60–250 kJ mol−1),43 indicating that it was easier for CoAl-1 to activate PMS compared to other reported catalysts.

3.4 Reusability of CoAl-1

The reusability of CoAl-1 was essential for its potential applications and was evaluated by reuse tests in this study. CoAl-1 particles were collected from the solution with an external magnetic field and reused under the same experimental conditions. Fig. 7a shows that the MG degradation efficiency was nearly 93.1% after 15 min in the first recycle process, and was 89.4%, 83.2% and 76.6% for the other three recycles. According to the pseudo-first-order kinetic model, the apparent rate constant (k) for the four recycles was estimated to be 0.1767, 0.1544, 0.1233, and 0.1022 min−1. In addition, the cobalt leaching amount among these cycles was tracked by ICP-MS. As shown in Fig. 7b, the cobalt leaching amount was quite low in the range of 36–57 μg L−1, which is far below the maximum allowable discharge quantity of cobalt (1 mg L−1) in water. The above results indicate that CoAl-1 exhibited desirable stability and reusability with a negligible decrease after four cycle runs. The negligible decrease of the catalyst activity might be ascribed to the accumulation of products or intermediates on the catalyst during the RhB degradation process and cobalt leaching from the catalyst in the four recycling processes.
image file: d3ra04575g-f7.tif
Fig. 7 (a) Reusability of CoAl-1 for RhB degradation; (b) the amount of leached Co ions during the successive runs. [Reaction conditions: [RhB] = 80 mg L−1, [PMS] = 0.3 mM, [catalyst] = 100 mg L−1, T = 298 K, and pH = 7.]

3.5 Catalytic mechanism for MB removal

To shed light on the reaction mechanism, the formation of reactive oxygen species in the CoAl-1/PMS system was investigated by EPR spectra. As shown in Fig. 8a and b, the strong quadruple peaks with an intensity ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]2[thin space (1/6-em)]:[thin space (1/6-em)]2[thin space (1/6-em)]:[thin space (1/6-em)]1 were the characteristic peaks of the DMPO–OH adducts, while the weaker peaks were assigned to the DMPO–SO4 adducts. The results demonstrated the formation of ˙SO4and ˙OH in the CoAl-1/PMS system. As previously reported, Co(II) could activate PMS to produce ˙SO4,44–46 while DMPO–SO4 adduct or ˙SO4could be easily transformed into DMPO–OH or ˙OH,47–49 thus the signal of ˙SO4 was weak. In addition, the significant signal of the TMP–1O2 adduct was observed, which had three characteristic peaks with equal intensity. These results confirmed the presence of ˙OH, ˙SO4, and 1O2 in the CoAl-1/PMS system.
image file: d3ra04575g-f8.tif
Fig. 8 ESR spectra of (a) Temp–1O2 and (b) DMPO adducts in the (DMPO–˙OH image file: d3ra04575g-u1.tif, DMPO–SO4˙ image file: d3ra04575g-u2.tif); the influence of scavengers on the degradation of RhB: (c) degradation efficiency and (d) rate constant; [reaction conditions: [RhB] = 80 mg L−1, [catalyst] = 100 mg L−1, [PMS] = 0.3 mM, T = 298 K, pH = 7 (unadjusted), [TBA] = [MA] = [p-BQ] = [FFA] = 2 mM].

To further identify the contributions of ROS to RhB degradation, a series of quenching experiments were conducted, in which MeOH was used as a scavenger for ˙SO4 and ˙OH, while TBA, p-BQ and FFA were chosen to quench ˙OH, ˙O2, and 1O2, respectively.50 As shown in Fig. 8c and d, p-BQ and TBA had little inhibitory effect on RhB degradation. When excess TBA and p-BQ were introduced separately into the CoAl-1/PMS system, RhB destruction efficiencies were slightly reduced from 93.1% to 72.2% and 82.2%, and the corresponding kobs values decreased by 39.1% and 20.2% respectively within 15 min, proving that ˙OH and ˙O2 played a negligible role in the destruction of RhB. Conversely, RhB degradation could be significantly inhibited by MeOH and FFA. When an excess of MeOH and FFA were added to the system, RhB degradation efficiency was sharply reduced to 26.2% and 14.3% from 93.1% of the blank test and the corresponding kobs values decreased by 83.1% and 92.3%, respectively. These results indicated that 1O2 dominated RhB degradation over the CoAl-1/PMS system, while ˙OH, ˙O2, and ˙SO4 could mainly serve as the intermediate for the generation of 1O2 and were indirectly involved in the degradation of RhB. Furthermore, ˙SO4 could be the dominant source of 1O2 and play an important role in RhB degradation.

Based on the above discussions, a possible mechanism for RhB degradation on CoAl-1 catalysts is proposed: on the one hand, the surface oxygen vacancy of the catalyst could serve as the active sites to mediate PMS to produce 1O2 (eqn (R1))

 
HSO5 + SO52− → HSO4 + SO42− + 1O2 (R1)

On the other hand, the Co2+/Co3+ redox cycle on the surface of CoAl-1 could activate PMS to provide a significant amount of ˙SO4 and ˙SO5 (eqn (R2) and (R3)). Subsequently, partial ˙SO4 reacted with H2O or OH from the solution to form HO˙ and O2 (eqn (R4)). The generated O2 received electrons and formed O2˙, which tended to convert into 1O2 (eqn (R5)–(R8)). Meanwhile, ˙SO4 and HO˙ reacted with PMS to produce ˙SO5, which could be converted into ˙SO4 and 1O2 (eqn (R9)–(R11)). Finally, under the strong oxidation of 1O2, RhB is quickly decomposed into CO2 and H2O eqn (R12).

 
Co3+ + HSO5 → Co2+ + SO5˙ + H+ (R2)
 
Co2+ + HSO5 → Co3+ + ˙SO4 + OH (R3)
 
2˙SO4 + 2OH → 2SO42− + 2˙OH + O2 (R4)
 
O2 + e → ˙O2 (R5)
 
˙O2 + ˙OH → 1O2 (R6)
 
˙OH + ˙OH → H2O + 1O2 (R7)
 
2O2˙ + 2H+1O2 + H2O2 (R8)
 
˙SO4 + HSO5 → ˙SO5 + SO42− + 2H+ (R9)
 
˙OH + HSO5 → ˙SO5 + H2O (R10)
 
2˙SO5 → ˙SO4 O2 ˙SO4 → 2˙SO4 + 1O2 (R11)
 
1O2 + RhB → CO2 + H2O + … (R12)

4. Conclusion

In this study, we successfully exfoliated the pristine bulk CoAl-LDHs into CoAl-LDHs nanosheets by a simple hydrothermal method in a KOH solution. The as-obtained CoAl-LDH nanosheets exhibited remarkable catalytic performance as a PMS activator for rhodamine B (RhB) degradation with the reaction rate constant (0.1687 min−1), which was nearly 2.22, 3.63, and 5.02 times that of CoAl-W, nano-Co3O4 and bulk CoAl-LDH, respectively. The superior performance was attributed to the nanosheet structure with more surface-exposed metal atoms and oxygen vacancies. A systematic analysis of the effects of reaction parameters indicated that the maximum RhB degradation was achieved under the conditions: catalyst dose 0.1 g L−1, PMS concentration 0.3 mM, pH 7, and temperature 298 K. Further analysis using electron paramagnetic resonance (EPR) and a series of scavenger experiments revealed that singlet oxygen (1O2) dominated RhB degradation during PMS activation, while ˙OH, ˙O2, ˙SO4 mainly served as intermediates for the generation of 1O2 and played an indirect role in oxidizing RhB. Overall, this study provides a simple method to fabricate LDH nanosheets used as PMS activators for enhanced water remediation.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by Hubei Key Laboratory of Animal Nutrition and Feed Science, Wuhan Polytechnic University (No. 201911), the building project of Hubei Province for Technology Innovation and Entrepreneurship Service Capacity (No. 2018BEC466), and the Central Committee Guides Local Science and Technology Development Special Project of Hubei Province (No. 2019ZYYD059).

Notes and references

  1. S. D. Richardson and T. A. Ternes, Water analysis: emerging contaminants and current issues, Anal. Chem., 2018, 90, 1398–1428 CrossRef PubMed.
  2. C. G. Daughton and T. A. Ternes, Pharmaceuticals and personal care products in the environment: agents of subtle change?, Environ. Health Perspect., 1999, 107, 907–938 CrossRef CAS PubMed.
  3. M. Ahmadi and F. Ghanbari, Organic dye degradation through peroxymonosulfate catalyzed by reusable graphite felt/ferriferrous oxide: mechanism and identification of intermediates, Mater. Res. Bull., 2019, 111, 43–52 CrossRef CAS.
  4. W. Li, P. X. Wu, Y. Zhu, Z. J. Huang, Y. H. Lu, Y. W. Li, Z. Dang and N. W. Zhu, Catalytic degradation of bisphenol A by CoMnAl mixed metal oxides catalyzed peroxymonosulfate: performance and mechanism, Chem. Eng. J., 2015, 279, 93–102 CrossRef CAS.
  5. J. Cao, L. Lai, B. Lai, G. Yao, X. Chen and L. Song, Degradation of tetracycline by peroxymonosulfate activated with zero-valent iron: performance, intermediates, toxicity and mechanism, Chem. Eng. J., 2019, 364, 45–56 CrossRef CAS.
  6. B. Chen, Z. Chen and S. Lv, A novel magnetic biochar efficiently sorbs organic pollutants and phosphate, Bioresour. Technol., 2011, 102(2), 716–772 CrossRef CAS PubMed.
  7. M. Wei, Y. Ruan, S. Luo, X. Li, A. Xu and P. Zhang, The facile synthesis of a magnetic OMS-2 catalyst for decomposition of organic dyes in aqueous solution with peroxymonosulfate, New J. Chem., 2015, 39(8), 6395–6403 RSC.
  8. B. Jiang, C. Jing, Y. Yuan, L. Feng, X. Liu, F. Dong, B. Dong and Y. X. Zhang, 2D-2D growth of NiFe LDH nanoflakes on montmorillonite for cationic and anionic dye adsorption performance, J. Colloid Interface Sci., 2019, 540, 398–409 CrossRef PubMed.
  9. M. Tian, S. S. Thind, J. S. Dondapti, X. Li and A. Chen, Electrochemical oxidation of 4- chlorophenol for wastewater treatment using highly active UV treated TiO2 nanotubes, Chemosphere, 2018, 209, 182–190 CrossRef CAS PubMed.
  10. J. Lee, U. von Gunten and J. H. Kim, Persulfate-based advanced oxidation: critical assessment of opportunities and roadblocks, Environ. Sci. Technol., 2020, 54, 3064–3081 CrossRef CAS PubMed.
  11. J. Wang and S. Wang, Activation of persulfate (PS) and peroxymonosulfate (PMS) and application for the degradation of emerging contaminants, Chem. Eng. J., 2018, 334, 1502–1517 CrossRef CAS.
  12. Y. Ji, C. Dong, D. Kong, J. Lu and Q. Zhou, Heat-activated persulfate oxidation of atrazine: implications for remediation of groundwater contaminated by herbicides, Chem. Eng. J., 2015, 263, 45–54 CrossRef CAS.
  13. F. Rehman, M. Sayed, J. A. Khan, N. S. Shah, H. M. Khan and D. D. Dionysiou, Oxidative removal of brilliant green by UV/S2O82-, UV/HSO5- and UV/H2O2 processes in aqueous media: a comparative study, J. Hazard. Mater., 2018, 357, 506–514 CrossRef CAS PubMed.
  14. Q. Zhao, Q. Mao, Y. Zhou, J. Wei, X. Liu, J. Yang, L. Luo, J. Zhang, H. Chen, H. Chen and L. Tang, Metal-free carbon materials-catalyzed sulfate radical-based advanced oxidation processes: a review on heterogeneous catalysts and applications, Chemosphere, 2017, 189, 224–238 CrossRef CAS PubMed.
  15. M. Kohantorabi, M. Hosseinifard and A. Kazemzadeh, Catalytic activity of a magnetic Fe2O3@CoFe2O4 nanocomposite in peroxymonosulfate activation for norfloxacin removal, New J. Chem., 2020, 44(10), 4185–4198 RSC.
  16. C. Tan, X. Lu, X. Cui, X. Jian, Z. Hu, Y. Dong, X. Liu, J. Huang and L. Deng, Novel activation of peroxymonosulfate by an easily recyclable VC@Fe3O4 nanoparticles for enhanced degradation of sulfadiazine, Chem. Eng. J., 2019, 363, 318–328 CrossRef CAS.
  17. G. Xian, G. Zhang, H. Chang, Y. Zhang, Z. Zou and X. Li, Heterogeneous activation of persulfate by Co3O4-CeO2 catalyst for diclofenac removal, J. Environ. Manage., 2019, 234, 265–272 CrossRef CAS PubMed.
  18. Z. Li, K. Liu, K. Fan, Y. Yang, M. Shao, M. Wei and X. Duan, Active-oxygen enhanced homogeneous nucleation of lithium metal on ultrathin layered double hydroxide, Angew. Chem., 2019, 58, 3962–3966 CrossRef CAS PubMed.
  19. Q. Wang, L. F. Chen, S. L. Guan, X. Zhang, B. Wang, X. Z. Cao, Z. Yu, Y. F. He, D. G. Evans, J. T. Feng and D. Q. Li, Ultrathin and Vacancy-Rich CoAl-Layered Double Hydroxide/Graphite Oxide Catalysts: Promotional Effect of Cobalt Vacancies and Oxygen Vacancies in Alcohol Oxidation, ACS Catal., 2018, 8(4), 3104–3115 CrossRef CAS.
  20. L. Huang, C. Megías-Sayago, R. Bingre, Q. Zheng, Q. Wang and B. Louis, Catalytic performance of layered double hydroxides (LDHs) derived materials in gas-solid and liquid-solid phase reactions, ChemCatChem, 2019, 11, 3279–3286 CrossRef CAS.
  21. G. Fan, F. Li, D. G. Evans and X. Duan, Catalytic applications of layered double hydroxides: recent advances and perspectives, Chem. Soc. Rev., 2014, 43, 7040–7066 RSC.
  22. J. A. Sun, L. X. Wang, Y. G. Wang, W. Y. Lv and Y. Y. Yao, Activation of peroxymonosulfate by MgCoAl layered double hydroxide: potential enhancement effects of catalyst morphology and coexisting anions, Chemosphere, 2022, 286, 131640–131650 CrossRef CAS PubMed.
  23. M. Kohantorabi, G. Moussavi and S. Giannakis, A review of the innovations in metal and carbon-based catalysts explored for heterogeneous peroxymonosulfate (PMS) activation, with focus on radical vs. non-radical degradation pathways of organic contaminants, Chem. Eng. J., 2021, 411, 127957–127983 CrossRef CAS.
  24. Y. Zong, K. Li, R. Tian, Y. Lin and C. Lu, Highly dispersed layered double oxide hollow spheres with sufficient active sites for adsorption of methyl blue, Nanoscale, 2018, 10, 23191–23197 RSC.
  25. R. Z. Ma, Z. P. Liu, L. Li, N. Iyi and T. Sasaki, Exfoliating layered double hydroxides in formamide: a method to obtain positively charged nanosheets, J. Mater. Chem., 2006, 16, 3809–3813 RSC.
  26. J. F. Yu, J. J. Liu, A. Clearfield, J. E. Sims, M. T. Speiegle, S. L. Suib and L. Y. Sun, Synthesis of Layered Double Hydroxide Single-Layer Nanosheets in Formamide, Inorg. Chem., 2016, 55, 12036–12041 CrossRef CAS PubMed.
  27. R. N. Guo, Y. L. Zhu, X. W. Cheng, J. J. Li and J. C. Crittenden, Efficient degradation of lomefloxacin by Co-Cu-LDH activating peroxymonosulfate process: optimization, dynamics, degradation pathway and mechanism, J. Hazard. Mater., 2020, 399, 122966–122980 CrossRef CAS PubMed.
  28. Y. P. Zhang, H. F. Xu and S. Lu, Preparation and application of layered double hydroxide nanosheets, RSC Adv., 2021, 11, 24254–24281 RSC.
  29. B. Chen, Z. Zhang, S. K. Kim, S. G. Lee, J. W. Lee, W. Y. Kim and K. J. Yong, Ostwald Ripening Driven Exfoliation to Ultrathin Layered Double Hydroxides Nanosheets for Enhanced Oxygen Evolution Reaction, ACS Appl. Mater. Interfaces, 2018, 10(51), 44518–44526 CrossRef CAS PubMed.
  30. Y. Y. Wang, Y. Q. Zhang, Z. J. Liu, C. Xie, S. Feng, D. D. Liu, M. F. Shao and S. Y. Wang, Layered Double Hydroxide Nanosheets with Multiple Vacancies Obtained by Dry Exfoliation as Highly Efficient Oxygen Evolution Electrocatalysts, Angew. Chem., Int. Ed., 2017, 56, 5867–5871 CrossRef CAS PubMed.
  31. X. Zhang, Y. F. Zhao, Y. X. Zhao, R. Shi, G. I. N. Waterhouse and T. R. Zhang, A Simple Synthetic Strategy toward Defect-Rich Porous Monolayer NiFe-Layered Double Hydroxide Nanosheets for Efficient Electrocatalytic Water Oxidation, Adv. Energy Mater., 2019, 9, 1900881–1900888 CrossRef.
  32. Z. Liu, L. Teng, L. F. Ma, Y. Liu, X. Y. Zhang, J. L. Xue, M. Ikram, M. Ullah, L. Li and K. Y. Shi, Porous 3D flower-like CoAl-LDH nanocomposite with excellent performance for NO2 detection at room temperature, RSC Adv., 2019, 9, 21911–21921 RSC.
  33. S. D. Jiang, L. Song, W. R. Zeng, Z. Q. Huang, J. Zhan, A. A. Stec, T. R. Hull, Y. Hu and W. Zhao, Self-Assembly Fabrication of Hollow Mesoporous Silica@CoAl Layered Double Hydroxide@Graphene and Application in Toxic Effluents Elimination, ACS Appl. Mater. Interfaces, 2015, 7, 8506–8514 CrossRef CAS PubMed.
  34. M. Zhang, Y. Liu, B. Liu, Z. Chen, H. Xu and K. Yan, Trimetallic NiCoFe-layered double hydroxides nanosheets efficient for oxygen evolution and highly selective oxidation of biomass-derived 5-hydroxymethylfurfural, ACS Catal., 2020, 10, 5179–5189 CrossRef CAS.
  35. H. Li, H. Wang, Q. Gao, B. Han, K. Xia and C. Zhou, Hierarchical flower-like Co2TiO4 nanosheets with unique structural and compositional advantages to boost peroxymonosulfate activation for degradation of organic pollutants, J. Mater. Chem. A, 2020, 8(40), 20953–20962 RSC.
  36. W. D. Oh, S. K. Lua, Z. Dong and T. T. Lim, Performance of magnetic activated carbon composite as peroxymonosulfate activator and regenerable adsorbent via sulfate radical-mediated oxidation processes, J. Hazard. Mater., 2015, 284, 1–9 CrossRef CAS PubMed.
  37. Z. D. Li, D. F. Liu, Y. X. Zhao, S. R. Li, X. C. Wei, F. S. Meng, W. L. Huang and Z. F. Lei, Singlet oxygen dominated peroxymonosulfate activation by CuO-CeO2 for organic pollutants degradation: performance and mechanism, Chemosphere, 2019, 233, 549–558 CrossRef CAS PubMed.
  38. J. Yan, J. Li, J. Peng, H. Zhang, Y. Zhang and B. Lai, Efficient degradation of sulfamethoxazole by the CuO@Al2O3 (EPC) coupled PMS system: optimization, degradation pathways and toxicity evaluation, Chem. Eng. J., 2019, 359, 1097–1110 CrossRef CAS.
  39. H. T. Li, Q. Gao, G. H. Wang, B. Han, K. H. Xia, J. P. Wu, C. G. Zhou and J. Dong, Postsynthetic incorporation of catalytically inert Al into Co3O4 for peroxymonosulfate activation and insight into the boosted catalytic performance, Chem. Eng. J., 2021, 426, 131292–131302 CrossRef CAS.
  40. C. Tan, X. Lu, X. Cui, X. Jian, Z. Hu, Y. Dong, X. Liu, J. Huang and L. Deng, Novel activation of peroxymonosulfate by an easily recyclable VC@Fe3O4 nanoparticles for enhanced degradation of sulfadiazine, Chem. Eng. J., 2019, 363, 318–328 CrossRef CAS.
  41. H. Li, Q. Gao, G. Wang, B. Han, K. Xia and C. Zhou, Architecturing CoTiO3 overlayer on nanosheets-assembled hierarchical TiO2 nanospheres as a highly active and robust catalyst for peroxymonosulfate activation and metronidazole degradation, Chem. Eng. J., 2020, 392, 123819 CrossRef CAS.
  42. M. Ding, W. Chen, H. Xu, Z. Shen, T. Lin, K. Hu, Ch. Lu and Z. Xie, Novel α-Fe2O3/MXene nanocomposite as heterogeneous activator of peroxymonosulfate for the degradation of salicylic acid, J. Hazard. Mater., 2020, 382, 121064 CrossRef CAS PubMed.
  43. H. Li, Q. Gao, G. Wang, B. Han, K. Xia and C. Zhou, Fabricating yolk–shell structured CoTiO3@ Co3O4 nanoreactor via a simple self-template method toward high performance peroxymonosulfate activation and organic pollutant degradation, Appl. Surf. Sci., 2021, 536, 147787 CrossRef CAS.
  44. M. Kohantorabi, G. Moussavi and S. Giannakis, A review of the innovations in metaland carbon-based catalysts explored for heterogeneous peroxymonosulfate (PMS) activation, with focus on radical vs. non-radical degradation pathways of organic contaminants, Chem. Eng. J., 2020, 411, 127957 CrossRef.
  45. M. M. Mian, G. Liu, B. Fu and Y. Song, Facile synthesis of sludge-derived MnOx-Nbiochar as an efficient catalyst for peroxymonosulfate activation, Appl. Catal., B, 2019, 255, 117765 CrossRef CAS.
  46. Q. F. Zhong, Q. T. Lin, R. L. Huang, H. Y. Fu, X. F. Zhang, H. Y. Luo and R. B. Xiao, Oxidative degradation of tetracycline using persulfate activated by N and Cu codoped biochar, Chem. Eng. J., 2020, 380, 122608–122618 CrossRef CAS.
  47. S. S. Yang, S. X. Zhang, X. Li, Y. X. Du, Y. X. Xing, Q. Xu, Z. H Wang, L. Li and X. T. Zhua, One-step pyrolysis for the preparation of sulfur doped biochar loaded with iron nanoparticles as an effective peroxymonosulfate activator for RhB degradation, New J. Chem., 2022, 46, 5678–5689 RSC.
  48. Y. Ren, L. Lin, J. Ma, J. Yang, J. Feng and Z. Fan, Sulfate radicals induced from peroxymonosulfate by magnetic ferrospinel MFe2O4 (M = Co, Cu, Mn, and Zn) as heterogeneous catalysts in the water, Appl. Catal., B, 2015, 165, 572–578 CrossRef CAS.
  49. L. Wu, Q. Zhang, J. Hong, Z. Dong and J. Wang, Degradation of bisphenol A by persulfate activation via oxygen vacancy-rich CoFe2O4-x, Chemosphere, 2019, 221, 412–422 CrossRef CAS PubMed.
  50. L. J. Rao, Y. F. Yang, L. K. Chen, X. D. Liu, H. X. Chen, Y. Y. Yao and W. T. Wang, Highly efficient removal of organic pollutants via a green catalytic oxidation system based on sodium metaborate and peroxymonosulfate, Chemosphere, 2020, 238, 124687 CrossRef CAS PubMed.

Footnote

Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ra04575g