Evolution of the surface atomic structure of multielement oxide films: curse or blessing?

Giada Franceschi *a, Renè Heller b, Michael Schmid a, Ulrike Diebold a and Michele Riva a
aInstitute of Applied Physics, TU Wien, Wiedner Hauptstraβe 8-10/E134, 1040, Vienna, Austria. E-mail: franceschi@iap.tuwien.ac.at
bInstitute of Ion Beam Physics and Materials Research, Helmholtz-Zentrum Dresden-Rossendorf e.V., Bautzner Landstraße 400, 01328, Dresden, Germany

Received 2nd October 2023 , Accepted 2nd November 2023

First published on 2nd November 2023


Abstract

Atomically resolved scanning tunneling microscopy (STM) and X-ray photoelectron spectroscopy (XPS) are used to gain atomic-scale insights into the heteroepitaxy of lanthanum–strontium manganite (LSMO, La1−xSrxMnO3−δ, x ≈ 0.2) on SrTiO3(110). LSMO is a perovskite oxide characterized by several composition-dependent surface reconstructions. The flexibility of the surface allows it to incorporate nonstoichiometries during growth, which causes the structure of the surface to evolve accordingly. This happens up to a critical point, where phase separation occurs, clusters rich in the excess cations form at the surface, and films show a rough morphology. To limit the nonstoichiometry introduced by non-optimal growth conditions, it proves useful to monitor the changes in surface atomic structures as a function of the PLD parameters and tune the latter accordingly.


1. Introduction

Perovskite oxides dominate a host of established and emerging technologies due to their extraordinary tunability.1–4 Characterized by the chemical formula ABO3, perovskites and related crystal structures can accommodate about 30 elements on the A site and over half the periodic table on the B site.5 This opens up the attractive possibility to control the interplay between spin, charge, orbital, and lattice degrees of freedom and achieve unique properties.3 One example is La1−xSrxMnO3−δ (lanthanum–strontium manganite, LSMO), which shows doping-dependent transitions from metal to insulator and from (anti)ferro- to paramagnetic, as well as interesting catalytic properties.6–10

Because of their high sensitivity to stoichiometry and crystal structure changes,11 the properties of perovskite oxides are best explored by working with single-crystalline samples or bulk-like epitaxial thin films. The growth of ideal perovskite-oxide films is challenging, however. In pulsed laser deposition (PLD) – the technique of choice for multielement oxides – many parameters can affect preferentially one element or another in the compound. These parameters include the laser energy density, spot size, pulse duration, deposition geometry, pressure and nature of the ambient gas, and deposition rate.12–15 Depending on the precise values of the deposition parameters (sometimes hard to reproduce in different laboratories13,16,17), elements may be preferentially ablated at the target, preferentially scattered by the background gas, and have preferential sticking to the substrate.13 Put simply, stoichiometric targets do not warrant stoichiometric films. The crystallinity, morphology, and other macroscopic properties are also influenced. The effects are more pronounced at thicknesses larger than a few nanometres. LSMO films exemplify the struggle. Their morphology, composition, transport, and magnetic properties are highly sensitive to the growth conditions.16,18–24 Crystalline precipitates during nonstoichiometric growth are common.25,26

The causes for morphological roughening are numerous and intertwined. In the simple case of one-component films, deposition rate, energetics, attachment kinetics at step edges, mechanical stress, angle dependent rate, capillarity, viscous flow, and nucleation are known to be relevant.27–32 These effects are expected to play a role also within the growth of perovskite oxides. This work demonstrates that additional effects – not considered in traditional models and related to the surface atomic details of the growing films – are important for understanding and controlling the complex growth behaviours of perovskite oxides.

Perovskite oxides are known to exhibit a host of composition-dependent atomic-scale surface structures (also named surface reconstructions).33–40 Previous studies on SrTiO3(110) have already shown that these reconstructions are critically important during epitaxial film growth. If the deposition parameters are not optimized and the growth is nonstoichiometric, excess cations can segregate to the film surface39 and alter its atomic structure. The nonstoichiometry of the deposited material might be minute but its influence on the surface atomic structure can be detected by reflection high-energy electron diffraction (RHEED),41 low-energy electron diffraction (LEED), and scanning tunneling microscopy (STM).39 Importantly, these changes can alter the growth mechanisms42,43 and the surface morphology: if reconstructions with different sticking properties develop and coexist on the surface, pits might develop on the low-sticking areas.13

The existence of surface reconstructions does not solely bring negative implications. As it was shown for SrTiO3,39 it also opens up attractive opportunities. In cases where all the introduced non-stoichiometry segregates to the surface of the growing film, optimal growth conditions and stoichiometric growth with virtually unlimited accuracy can be achieved by monitoring the changes in the surface atomic structure as a function of film thickness and deposition parameters.39

This work builds on previous studies on SrTiO3 homoepitaxy. It focuses on LSMO films deposited on well-defined SrTiO3(110) substrates (see Section S1 of the ESI for details on the setups and the growth) ref. 58. It investigates how the surface atomic structures of LSMO evolve during growth as a function of different parameters and film thicknesses, and how to leverage such changes to optimize the deposition parameters. The concepts are showcased by depositing under controlled conditions, where one parameter at a time is carefully modified – in this case, the value of the O2 background pressure (pO2) within the incongruent transfer regime, where the lighter Mn species scatter more than the heavier La and Sr, leading to enrichment in La and Sr (Mn) at higher (lower) O2 pressures. The surface evolution is monitored with XPS and STM. Akin to SrTiO3, non-stoichiometries shift the surface atomic structure along established surface phase diagrams, following their substantial segregation to the surface.40,44 When the excess material cannot be accommodated by a suitable surface reconstruction, it precipitates in the form of clusters rich in the excess cations. Nonetheless, appropriate ultrahigh vacuum (UHV)-based surface treatments can heal the surface. A method is presented to optimize the PLD parameters to grow high-quality multielement films. Different from typical practices, it does not rely on ex-situ, post-mortem, bulk analyses. Rather, it leverages the changes in surface atomic structure that follow the partial segregation of non-stoichiometry. Ex-situ bulk analyses are offered to support the quality of the films and provide a link with standard characterization techniques.

2. Insights into the growth of LSMO(110)

This section addresses the role of pO2 during PLD on the morphology and composition of LSMO(110) films. Fig. 1a–c show the STM morphology of three thin films grown at pO2 values ranging between 5 × 10−3 mbar and 0.2 mbar (all other parameters are nominally the same: 1 Hz laser repetition rate, 1.9 J cm−2 laser fluence, 700 °C substrate temperature). All films have the same thickness of ≈2.5 nm or 9 layers, where one layer corresponds to the separation between two (110) planes, ≈0.276 nm.
image file: d3na00847a-f1.tif
Fig. 1 Effect of pO2 during PLD on the morphology and composition of LSMO(110) films. (a–c) Top row: 300 × 300 nm2 STM images (Vsample = +2 V, Itunnel = 0.2 nA) of thin films (9 layers, ≈ 2.5 nm thickness) grown at 1 Hz, 1.9 J cm−2, 700 °C, and 5 × 10−3 mbar ≤ pO2 ≤ 0.2 mbar; bottom row: 15 × 15 nm2 STM images, high-pass-filtered for displaying purposes. (d) XPS intensity ratios of Mn 2p, La 4d, and Sr 3d peaks as a function of pO2; lower pO2 yields Mn-richer surfaces (the analysis includes an additional datapoint of a 9-layer-thick film grown at 5 × 10−6 mbar). Note that the Sr signal originating from the substrate cannot be decoupled from the one in the film.

In Fig. 1, all films appear atomically flat on the scale of a few hundred nanometres (top row). On a smaller scale (bottom row), different surface structures with different periodicities (i.e., different surface reconstructions) are evident. The same reconstructions were observed by depositing sub-monolayer amounts of Mn on a stoichiometric film in order to establish a quantitative surface phase diagram of LSMO(110).44 Comparing this phase diagram with Fig. 1 reveals that the films grown at lower pressures exhibit reconstructions richer in Mn. This is confirmed by the XPS analysis of Fig. 1d. Note that the variation of the Mn/La XPS intensity ratio (Fig. 1d) by more than a factor of 1.6 is much higher than what would be possible in perovskite-type LSMO according to the bulk phase diagram.45 While STM shows different surface reconstructions (Fig. 1a–c), all these surface phases are based on the same perovskite lattice of the underlying layers.44 There is no evidence for the formation of different phases in the deeper layers of these films. This indicates that the stoichiometry variations at the surface are larger than in the deeper layers of the film.

Fig. 2 displays the intensity of the specular RHEED spot versus the deposition time for three pO2 values. All depositions occur in a layer-by-layer mode (one RHEED oscillation equals one layer). Higher pressures produce longer periods, an indication that less material reaches the substrate. Moreover, the intensities of the minima and maxima differ for the three films. This is not necessarily always an indication for better or worse layer-by-layer growth, however. The different surface reconstructions developing during growth (Fig. 1) could potentially cause diffraction conditions different from the starting point, which may explain some amplitude variations of the intensity oscillations.13 Nevertheless, the more pronounced decay observed in Fig. 2a probably indicates the slightly rougher surface morphology of the corresponding film (observed in STM, not shown here).


image file: d3na00847a-f2.tif
Fig. 2 RHEED oscillations during the growth of thin LSMO(110) films (≈2.5 nm thick) at different pO2 (values indicated in the respective panels) and otherwise identical growth parameters (1 Hz, 1.9 J cm−2, 700 °C). Note that the data do not correspond to the same films as shown in Fig. 1.

Growing thicker films at the same conditions as in Fig. 1a–c induces dramatic morphology changes, see Fig. 3. The lowest and highest pressures (5 × 10−3 mbar, Fig. 3a; 0.2 mbar, Fig. 3c) produce new features a few nanometres in height, located mainly at the step edges and poorly conductive, as judged by the behaviour of STM. At the intermediate pressure of 4 × 10−2 mbar, the surface preserves its flatness up to a thickness of 132 nm. Note that the imperfect films shown in Fig. 3 are significantly thinner: clusters appear at thicknesses of only 5.5 and 11 nm in Fig. 3a and c, respectively.


image file: d3na00847a-f3.tif
Fig. 3 Accumulation of nonstoichiometry at the surface of LSMO(110) films. (a) 2.0 × 2.0 μm2 AFM image and (b and c) 300 × 300 nm2 STM images of LSMO(110) films thicker than those in Fig. 1 grown at different pO2 and otherwise identical deposition parameters as to Fig. 1. Nonstoichiometric growth conditions (a and c) result in poorly conductive, few nanometers-high features on the surface that are identified as manganese- and lanthanum-oxide-rich clusters at low and high pO2, respectively. Line scans over selected clusters are shown in the insets. (b) Ideal stoichiometry leads to films without precipitates even at a large thickness.

The bulk properties of films without clusters were characterized with RBS and XRD, see Fig. S1 and S2, ESI. The films are stoichiometric and crystalline. RBS quantified the composition as (La0.78±0.03Sr0.22±0.03)1.06±0.05MnO3, close to the target's (La0.79±0.02Sr0.21±0.02)0.96±0.08MnO3. The analysis of XRD reciprocal-space maps59–66 reveals that the films are crystalline but only partially relaxed – by 34.7% along [1[1 with combining macron]0] and 6% along [001]. This is expected for heteroepitaxial films under slight stress46 that relax by introducing misfit dislocations and forming mosaics. The residual deformation in the film in all three directions has an absolute value of less than 2 pm per unit cell. Best-fit lattice constants and angles are reported in Table S1 of the ESI.

Discussion

As mentioned in the Introduction, stoichiometric growth in PLD can be achieved following the optimization of many parameters,12 among others the oxygen background pressure and the laser fluence.47 As discussed below, both parameters are responsible for the growth behaviours summarized by Fig. 1 and 3.

Changes in the film composition as a function of pO2 in multi-element oxides can be explained within the three-pressure-regimes framework23,48,49 (regardless of the plume composition right after the ablation, which can be affected by the laser fluence, see below). At low-enough pO2, the ablated species are congruently transferred to the substrate. At intermediate pressures, lighter species are scattered more than heavier ones and the film becomes enriched with the heavier species as pO2 increases.50 At very high pO2, in the so-called shock-wave regime, all ablated species are slowed down equally; they are kept confined in the plume and transferred congruently to the substrate. These pressure regimes are identified not only by pO2 but also by the target-to-substrate distance16D (for the experimental setup used here, D = 55 mm). Here, the low-pressure regime occurs at pO2 ≤ 5 × 10−3 mbar: Below this value, there is no change in the XPS signals in Fig. 1, indicating congruent transfer. The intermediate pressure regime occurs at 3 × 10−2pO2 ≤ 0.2 mbar: the Mn content decreases with increasing pressure (Mn is the lightest cation in LSMO).

If the laser fluence is chosen such that all the species are ablated congruently at the target, the target has ideal stoichiometry, and the sticking probability of all ablated species on the surface is the same, it is possible to achieve near-ideal stoichiometries by depositing within either the low- or the high-pressure regimes. However, it is rare that all these conditions are fulfilled. Tiny deviations in the laser fluence or pulse duration can affect the ablation significantly, inducing the preferential ablation of one element over another in the multielement oxide. This is exemplified by the homoepitaxy of SrTiO3, where congruent ablation is achieved only within a very narrow window of laser fluence.13,17,39,51 Moreover, reproducing the laser fluence in different PLD setups is challenging:13 The spot size and the intensity distribution within the spot affect the deposition greatly;12 the most common way to adjust the UV pulse energy, by changing the discharge voltage of the UV laser, affects the pulse duration and beam divergences. Moreover, UV laser gases age over time, causing increasing pulse-to-pulse standard deviations and ill-defined fluences.

This work demonstrates how to achieve near-ideal stoichiometries even when the ablation is incongruent by exploiting the wider tunability window offered by the oxygen background pressure: the cation non-stoichiometry caused by preferential ablation can be mitigated by exploiting preferential scattering effects within the intermediate-pressure regime.

The “intermediate-pressure” film of Fig. 3b has a composition close to that of the target (see RBS analysis in Fig. S1c, ESI). Then, according to the XPS data in Fig. 1d, films grown at lower and higher pO2 (i.e., congruent transfer regimes) must be Mn rich and Mn deficient, respectively. This means that Mn is preferentially ablated at the target with the chosen laser fluence: Mn-rich films are obtained at low pO2 because the Mn-enriched plume is transferred congruently. The ideal stoichiometry is achieved at a specific value of intermediate pO2 where the excess Mn is scattered more than the heavy La species. Finally, at even higher pressures, more than the excess Mn is scattered away and the films grow La-rich. The preferential ablation of Mn at the target is possibly caused by the laser fluence being too low. Previous studies on SrTiO3 homoepitaxy have shown that low fluences produce Sr-rich films,52,53 probably because of the higher vapor pressure of Sr compared to Ti; similarly, Mn could be preferentially ablated at low laser fluences because of its higher vapor pressure compared to La.

The different film compositions translate into different atomic-scale surface structures (Fig. 1a–c). The changes in the RHEED patterns of LSMO films grown at different pO2 observed in the literature22 likely arise from the different surface reconstructions formed in each regime.

During SrTiO3(110) homoepitaxy, all non-stoichiometry segregates to the surface and changes its composition and atomic structure according to its composition phase diagrams.13,39 While it is not possible to prove that such full segregation occurs on LSMO(110) as well, several pieces of evidence support that segregation occurs at least partially, as seen by: (i) different surface structures forming on thin films with different compositions (Fig. 1), (ii) the evolution of the surface structures with increasing thickness (see Section 3), (iii) the XPS intensities mentioned in the previous paragraph, and (iv) the formation of non-conductive clusters when a critical thickness is overcome (Fig. 3). Since LSMO is an electrical conductor at room temperature, these clusters must consist of a different material. Hence, they are reasonably assigned to MnOx and LaOx excess introduced within the low- and high- pressure regimes, respectively. This is supported by the fact that similar clusters are observed after depositing large amounts (more than ≈2 ML) of Mn and La on well-defined LSMO(110) surfaces followed by short annealing times (≤20 min); and by the previously reported formation of MnOx precipitates in epitaxial LSMO(001) films under Mn-rich conditions.25

The 3D clusters form when the surface cannot accommodate the excess cations by modifying its atomic structure. It was already reported that Mn (La) species stick less on Mn(La)-richer surfaces.44 A careful inspection of the LaOx clusters in Fig. 3c reveals that they actually consist of pits surrounded by tall rims – similar to the features formed during the Ti-rich homoepitaxy of SrTiO3(110).13 There, the formation of pits was assigned to surface-dependent sticking and diffusion effects. The case of LSMO(110) appears similar. At La-rich conditions, the surface structure shifts towards La-rich reconstructions;44 at a critical composition, it becomes more favourable to nucleate and grow La-rich clusters than to incorporate more La in the surface structure.

Preferential sticking effects could act as a self-adjusting feedback mechanism for the film stoichiometry under slightly nonstoichiometric conditions: for slightly La-rich fluxes, the surface will gradually shift towards A-site richer reconstructions, onto which Mn sticks better, such that the surface shifts back towards Mn-richer structures. Now more La sticks, and so on. In principle, the forgiveness of this growth mechanism can allow growing atomically flat and stoichiometric films even under slightly nonstoichiometric conditions. However, as discussed above, this will work only up to a certain point: if the cation non-stoichiometry introduced by the incoming flux exceeds the capability of the surface to accommodate the non-stoichiometry via a change of the surface structure, oxide clusters form instead. One should also mention that, compared to SrTiO3(110), the surface reconstructions of LSMO(110) are separated by larger compositional differences.39,44 Hence, larger deposited non-stoichiometry can be accommodated at the surface of LSMO(110) films while yielding atomically flat films over a larger window of growth parameters.

One expects non-stoichiometry to accumulate at surfaces rather than in the bulk when forming bulk defects is comparatively more costly.39,54 Interestingly, the bulk phase diagrams of La0.8Sr0.2MnO3 (ref. 45) show that cation excesses are not easily incorporated in the bulk at UHV-compatible pressures. At atmospheric pressure, the system can accommodate significant excess of oxygen (and, possibly, cations). Nonetheless, our data show that excess Mn tends to float to the surface and change the surface atomic structure. Thus, non-stoichiometry segregation appears to be a powerful effect even in those perovskite oxides whose phase diagram would allow creating bulk defects.

3. Strategies to obtain ideal films

This section illustrates a strategy to pinpoint the optimal growth conditions for LSMO(110) films (in this case, the value of pO2 required to create a stoichiometric film in spite of the Mn-rich ablation). Several films were grown within the optimal range around 10−2 mbar (see Section 2). The corresponding surface structure changes were monitored with STM. Fig. 4 summarizes the results. For reference, the top row of Fig. 4 reports the surface phase diagram of LSMO(110) in the relevant pO2 range.44 Before each deposition, the surface was prepared to exhibit the ‘fishbone’ reconstruction of Fig. 4c, i.e., a image file: d3na00847a-t1.tif superstructure. This reconstruction as well as the other surface structures and their short-hand notation are described in ref. 44.
image file: d3na00847a-f4.tif
Fig. 4 Pinpointing the exact pO2 value for optimal LSMO(110) growth. (a–d) 12 × 12 nm2 STM images of selected surface structures of the surface phase diagram of LSMO(110),44 obtained by depositing controlled amounts of La or Mn from La2O3 and MnO targets in PLD plus annealing at 700 °C and 0.2 mbar O2 (see Methods section in the ESI; 1 ML corresponds to the number of Mn sites in an (AMnO)2 plane of LSMO(110), i.e., 4.64 × 1014 at. cm−2). (e–g) 70 × 70 nm2 STM images of LSMO films of various thicknesses grown at different pO2, always starting from LSMO(110) films with the fishbone structure of panel (c). (e) 5 nm-thick film grown at 2.0 × 10−2 mbar O2, displaying patches of the Mn-rich (m × 1) structure of panel (a). (f) 16 nm-thick film grown at 4.0 × 10−2 mbar O2, with a surface reconstruction in between the fishbone and (2 × 1). (g) 16 nm-thick film grown at 4.5 × 10−2 mbar O2, with patches of the (1 × 1) and of the fishbone reconstructions.

First, 5 nm were grown at 2.0 × 10−2 mbar O2. The surface (Fig. 4e) is atomically flat but exhibits patches of the (m × 1) structure of Fig. 4a, indicating that this pressure introduces a significant Mn excess. Indeed, when continuing growth at this oxygen pressure, MnOx-rich clusters are formed at 10 nm thickness (not shown).

As learned from Fig. 1, higher values of pO2 should introduce less Mn. By growing a film of 5 nm thickness at 4.0 × 10−2 mbar, the surface structure remains essentially the same as the starting point (not shown). Nonetheless, increasing the thickness to 16 nm (Fig. 4f) reveals a mix of the fishbone reconstruction (solid oval) and a reconstruction between the fishbone and the (2 × 1),44 indicating that the conditions are still Mn-enriching. Thus, the pressure should be increased further.

Growing 16 nm at pO2 = 4.5 × 10−2 mbar on SrTiO3 pushes the surface toward the other end of the surface phase diagram (Fig. 4g): patches of the (1 × 1) reconstruction of Fig. 4d (A-site richer than the fishbone) coexist with fishbone-reconstructed areas. However, these conditions are still not ideal: larger thicknesses produce increasing areal coverages of (1 × 1) followed by the formation of AOx-rich clusters.

The ideal condition is reached at 4.2 × 10−2 mbar. A film of 16 nm thickness shows a small (1 × 1) coverage (Fig. 5a). A flat surface is maintained up to 70 nm thickness (Fig. 5b).


image file: d3na00847a-f5.tif
Fig. 5 LSMO(110) film grown at optimized conditions. (a) 70 × 70 nm2 and (b) 500 × 500 nm2 STM images of 16 nm-thick and of 70 nm-thick LSMO(110) films, respectively, grown onto a fishbone-reconstructed LSMO(110) surface at 4.2 × 10−2 mbar O2. Both morphologies are atomically flat. At the atomic scale, (1 × 1) patches are visible [orange in panel (a)].

This section has shown how to grow flat films by detecting the non-stoichiometry from its influence on the surface reconstruction and adjusting pO2 accordingly. Notably, it is also possible to recover films with precipitates by means of appropriate UHV treatments. Section S3 of ESI shows that alternating annealing at oxidizing and reducing conditions favors surface diffusion and the flattening of the surface (as shown in ref. 55, this is a common behavior of oxide materials). This strategy is more effective than standard sputtering–annealing cycles.

4. Conclusions

This work addresses the correlation between non-stoichiometry (systematically tuned by varying the O2 background pressure), surface morphology, and surface atomic structures in PLD-grown LSMO(110) films by combining chemical analysis by XPS and atomically resolved STM. The often-overlooked surface atomic details have important implications for the growth. The surface can incorporate excess cations to a limited extent. In addition, the film composition may be influenced by preferential sticking. The composition-dependent surface atomic structures offer a precise metric to optimize the PLD parameters and achieve high-quality films. Since non-stoichiometries tend to segregate to the film surface and are prone to change its surface atomic structure, a stable atomic-scale surface structure at increasing film thicknesses indicates that the chosen PLD parameters yield a close-to-stoichiometric growth. On the other hand, a shift in the surface atomic structure indicates that cation excesses are introduced. To achieve close-to-stoichiometric films and avoid precipitation of undesired phases, the PLD parameters should be tuned such that the atomic-scale structure of the surface remains stable.

Monitoring the details of the surface atomic structures of the film also sheds light on previously disregarded mechanisms inducing morphological roughening. When the introduced non-stoichiometry exceeds a critical value, the surface cannot accommodate the excess cations by changing its atomic structure anymore. Instead, clusters of the excess material develop at the surface. In such cases, alternating annealing treatments at oxidizing and reducing conditions is an effective means to remediate the surface morphology.

Many phenomena observed during the growth of LSMO(110), including non-stoichiometry segregation that alters the surface structure, surface-dependent incorporation of deposited cations, and phase separation, seem to be a general trait of perovskite oxides and possibly many other multi-element compounds.13,14,56,57 A growing number of systems is reported to exhibit composition-related surface reconstructions with an apparent tendency to accommodate cation excesses. The authors contend that the findings reported here reflect general behaviours of complex oxide films, independent of the growth technique. The insights and methods presented can guide the growth optimization of perovskite-oxide films.

Author contributions

Conceptualization: GF and MR. Investigation: GF, MR and RH. Validation: MR, MS and UD. Supervision: MR, MS and UD. Funding acquisition: UD. Writing, original draft: GF. Writing, review and editing: all authors.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

The authors were supported by the Austrian Science Fund (FWF) through project SFB-F81 “Taming Complexity in materials modeling” (TACO) and by the European Research Council (ERC) under the European Union's Horizon 2020 research and innovation programme (grant agreement No. 883395, Advanced Research Grant ‘WatFun’).

Notes and references

  1. P. Zubko, S. Gariglio, M. Gabay, P. Ghosez and J. M. Triscone, Interface physics in complex oxide heterostructures, Annu. Rev. Condens. Matter Phys., 2011, 2, 141–165,  DOI:10.1146/annurev-conmatphys-062910-140445.
  2. A. S. Bhalla, R. Guo and R. Roy, The perovskite structure – A review of its role in ceramic science and technology, Mater. Res. Innovations, 2000, 4, 3–26,  DOI:10.1007/s100190000062.
  3. M. A. Peña and J. L. G. Fierro, Chemical structures and performance of perovskite oxides, Chem. Rev., 2001, 101, 1981–2017,  DOI:10.1021/cr980129f.
  4. D. P. Kumah, J. H. Ngai and L. Kornblum, Epitaxial oxides on semiconductors: from fundamentals to new devices, Adv. Funct. Mater., 2020, 30, 1901597,  DOI:10.1002/adfm.201901597.
  5. D. G. Schlom, L. Q. Chen, X. Pan, A. Schmehl and M. A. Zurbuchen, A thin film approach to engineering functionality into oxides, J. Am. Ceram. Soc., 2008, 91, 2429–2454,  DOI:10.1111/j.1551-2916.2008.02556.x.
  6. J. Junquera and P. Ghosez, Critical thickness for ferroelectricity in perovskite ultrathin films, Nature, 2003, 422, 506–509,  DOI:10.1038/nature01501.
  7. Z. Liao and J. Zhang, Metal-to-insulator transition in ultrathin manganite heterostructures, Appl. Sci., 2019, 9, 144,  DOI:10.3390/app9010144.
  8. J. Hemberger, A. Krimmel, T. Kurz, H. A. Krug von Nidda, V. Y. Ivanov, A. A. Mukhin, A. M. Balbashov and A. Loidl, Structural, magnetic, and electrical properties of single-crystalline La1−xSrxMnO3 (0.4 < x < 0.85), Phys. Rev. B: Condens. Matter Mater. Phys., 2002, 66, 1–8,  DOI:10.1103/PhysRevB.66.094410.
  9. C. Sun, R. Hui and J. Roller, Cathode materials for solid oxide fuel cells: A review, J. Solid State Electrochem., 2010, 14, 1125–1144,  DOI:10.1007/s10008-009-0932-0.
  10. J. Hwang, R. R. Rao, L. Giordano, Y. Katayama, Y. Yu and Y. Shao-Horn, Perovskites in catalysis and electrocatalysis, Science, 2017, 358, 751–756,  DOI:10.1126/science.aam7092.
  11. R. Ramesh and D. G. Schlom, Creating emergent phenomena in oxide superlattices, Nat. Rev. Mater., 2019, 4, 257–268,  DOI:10.1038/s41578-019-0095-2.
  12. A. Ojeda-G-P, M. Döbeli and T. Lippert, Influence of plume properties on thin film composition in pulsed laser deposition, Adv. Mater. Interfaces, 2018, 5, 1701062,  DOI:10.1002/admi.201701062.
  13. M. Riva, G. Franceschi, M. Schmid and U. Diebold, Epitaxial growth of complex oxide films: Role of surface reconstructions, Phys. Rev. Res., 2019, 1, 33059,  DOI:10.1103/physrevresearch.1.033059.
  14. P. Schöffmann, S. Pütter, J. Schubert, W. Zander, J. Barthel, P. Zakalek, M. Waschk, R. Heller and T. Brückel, Tuning the Co/Sr stoichiometry of SrCoO2.5 thin films by RHEED assisted MBE growth, Mater. Res. Express, 2020, 7, 116404,  DOI:10.1088/2053-1591/abc58b.
  15. H. Schraknepper, C. Bäumer, F. Gunkel, R. Dittmann and R. A. De Souza, Pulsed laser deposition of SrRuO3 thin-films: The role of the pulse repetition rate, APL Mater., 2016, 4, 126109,  DOI:10.1063/1.4972996.
  16. M. Koubaa, A. M. Haghiri-Gosnet, R. Desfeux, P. Lecoeur, W. Prellier and B. Mercey, Crystallinity, surface morphology, and magnetic properties of La0.7Sr0.3MnO3 thin films: an approach based on the laser ablation plume range models, J. Appl. Phys., 2003, 93, 5227,  DOI:10.1063/1.1566093.
  17. T. Ohnishi, H. Koinuma and M. Lippmaa, Pulsed laser deposition of oxide thin films, Appl. Surf. Sci., 2006, 252, 2466,  DOI:10.1016/j.apsusc.2005.04.057.
  18. R. Bachelet, D. Pesquera, G. Herranz, F. Sánchez and J. Fontcuberta, Persistent two-dimensional growth of (110) manganite films, Appl. Phys. Lett., 2010, 97, 121904,  DOI:10.1063/1.3490713.
  19. H. Guo, D. Sun, W. Wang, Z. Gai, I. Kravchenko, J. Shao, L. Jiang, T. Z. Ward, P. C. Snijders, L. Yin, J. Shen and X. Xu, Growth diagram of La0.7Sr0.3MnO3 thin films using pulsed laser deposition, J. Appl. Phys., 2013, 113, 234301,  DOI:10.1063/1.4811187.
  20. E. Annese, T. J. A. Mori, P. Schio, B. R. Salles and J. C. Cezar, Influence of the growth parameters on the electronic and magnetic properties of La0.67Sr0.33MnO3 epitaxial thin films, Appl. Surf. Sci., 2018, 437, 281,  DOI:10.1016/j.apsusc.2017.12.164.
  21. J. X. Ma, X. F. Liu, T. Lin, G. Y. Gao, J. P. Zhang, W. B. Wu, X. G. Li and J. Shi, Interface ferromagnetism in (110)-oriented La0.7Sr0.3MnO3/SrTiO3 ultrathin superlattices, Phys. Rev. B: Condens. Matter Mater. Phys., 2009, 79, 174424,  DOI:10.1103/PhysRevB.79.174424.
  22. M. Huijben, L. W. Martin, Y.-H. Chu, M. B. Holcomb, P. Yu, G. Rijnders, D. H. A. Blank and R. Ramesh, Critical thickness and orbital ordering in ultrathin La0.7Sr0.3MnO3 films, Phys. Rev. B: Condens. Matter Mater. Phys., 2008, 78, 94413,  DOI:10.1103/PhysRevB.78.094413.
  23. J. Chen, M. Döbeli, D. Stender, K. Conder, A. Wokaun, C. W. Schneider and T. Lippert, Plasma interactions determine the composition in pulsed laser deposited thin films, Appl. Phys. Lett., 2014, 105, 114104,  DOI:10.1063/1.4895788.
  24. S. K. Chaluvadi, V. Polewczyk, A. Y. Petrov, G. Vinai, L. Braglia, J. M. Diez, V. Pierron, P. Perna, L. Mechin, P. Torelli and P. Orgiani, Electronic properties of fully strained La1-xSrxMnO3 thin films grown by molecular beam epitaxy (0.15 ≤ x ≤ 0.45), ACS Omega, 2022, 7, 14571–14578,  DOI:10.1021/acsomega.1c06529.
  25. A. Steffen, A. Glavic, T. Gutberlet, H. Ambaye, J. Schubert, S. Geprägs, J. Barthel, S. Mattauch, W. Zander, M. Kruth, P. Schöffmann, S. Pütter and T. Brückel, Unexpected precipitates in conjunction with layer-by-layer growth in Mn-enriched La2/3Sr1/3MnO3 thin films, Thin Solid Films, 2021, 735, 138862,  DOI:10.1016/J.TSF.2021.138862.
  26. Y. Ishii, H. Sato, A. Sawa, T. Yamada, H. Akoh, K. Endo, M. Kawasaki and Y. Tokura, Precipitate-free films of La1-xSrxMnO3 grown on the substrates with artificial step edges, Appl. Phys. Lett., 2004, 85, 3800–3802,  DOI:10.1063/1.1807969.
  27. M. Schmid, C. Lenauer, A. Buchsbaum, F. Wimmer, G. Rauchbauer, P. Scheiber, G. Betz and P. Varga, High island densities in pulsed laser deposition: Causes and implications, Phys. Rev. Lett., 2009, 103, 1–4,  DOI:10.1103/PhysRevLett.103.076101.
  28. J. H. Jeffries, J. K. Zuo and M. M. Craig, Instability of kinetic roughening in sputter-deposition growth of Pt on glass, Phys. Rev. Lett., 1996, 76, 4931–4934,  DOI:10.1103/PhysRevLett.76.4931.
  29. B. J. Spencer, S. H. Davis and P. W. Voorhees, Morphological instability in epitaxially strained dislocation-free solid films: Nonlinear evolution, Phys. Rev. B: Condens. Matter Mater. Phys., 1993, 47, 9760–9777,  DOI:10.1103/PhysRevB.47.9760.
  30. B. J. Palmer and R. G. Gordon, Kinetic model of morphological instabilities in chemical vapor deposition, Thin Solid Films, 1989, 177, 141–159,  DOI:10.1016/0040-6090(89)90563-4.
  31. A. Jamnig, D. G. Sangiovanni, G. Abadias and K. Sarakinos, Optimization of La0.7Ba0.3MnO3-δ complex oxide laser ablation conditions by plume imaging and optical emission spectroscopy, Sci. Rep., 2019, 9, 1–11,  DOI:10.1063/1.3467770.
  32. L. A. Zepeda-Ruiz, G. H. Gilmer, C. C. Walton, A. V. Hamza and E. Chason, Surface morphology evolution during sputter deposition of thin films – lattice Monte Carlo simulations, J. Cryst. Growth, 2010, 312, 1183–1187,  DOI:10.1016/j.jcrysgro.2009.12.035.
  33. D. Kienzle, P. Koirala and L. D. Marks, Lanthanum aluminate (110) 3×1 surface reconstruction, Surf. Sci., 2015, 633, 60,  DOI:10.1016/j.susc.2014.11.016.
  34. S. V. Levchenko and A. M. Rappe, Influence of ferroelectric polarization on the equilibrium stoichiometry of lithium niobate (0001) surfaces, Phys. Rev. Lett., 2008, 100, 256101,  DOI:10.1103/PhysRevLett.100.256101.
  35. S. Gerhold, Z. Wang, M. Schmid and U. Diebold, Stoichiometry-driven switching between surface reconstructions on SrTiO3(001), Surf. Sci., 2014, 621, L1–L4,  DOI:10.1016/j.susc.2013.10.015.
  36. A. M. Kolpak, D. Li, R. Shao, A. M. Rappe and D. A. Bonnell, Evolution of the structure and thermodynamic stability of the BaTiO3(001) surface, Phys. Rev. Lett., 2008, 101, 36102,  DOI:10.1103/PhysRevLett.101.036102.
  37. W. A. Saidi, J. M. P. Martirez and A. M. Rappe, Strong reciprocal interaction between polarization and surface stoichiometry in oxide ferroelectrics, Nano Lett., 2014, 14, 6711–6717,  DOI:10.1021/nl5035013.
  38. B. C. Russell and M. R. Castell, Surface of sputtered and annealed polar SrTiO3(111): TiOx-rich (n × n) reconstructions, J. Phys. Chem. C, 2008, 112, 6538–6545,  DOI:10.1021/jp711239t.
  39. M. Riva, G. Franceschi, Q. Lu, M. Schmid, B. Yildiz and U. Diebold, Pushing the detection of cation nonstoichiometry to the limit, Phys. Rev. Mater., 2019, 3, 43802,  DOI:10.1103/PhysRevMaterials.3.043802.
  40. G. Franceschi, M. Schmid, U. Diebold and M. Riva, Two-dimensional surface phase diagram of a multicomponent perovskite oxide: La0.8Sr0.2MnO3(110), Phys. Rev. Mater., 2021, 5, L092401,  DOI:10.1103/PhysRevMaterials.5.L092401.
  41. A. P. Kajdos and S. Stemmer, Surface reconstructions in molecular beam epitaxy of SrTiO3, Appl. Phys. Lett., 2014, 105, 191901,  DOI:10.1063/1.4901726.
  42. F. Sánchez, C. Ocal and J. Fontcuberta, Tailored surfaces of perovskite oxide substrates for conducted growth of thin films, Chem. Soc. Rev., 2014, 43, 2272–2285,  10.1039/c3cs60434a.
  43. Y. J. Chang and S.-H. Phark, Atomic-scale visualization of initial growth of perovskites on SrTiO3(001) using scanning tunneling microscope, Curr. Appl. Phys., 2017, 17, 640–656,  DOI:10.1016/j.cap.2016.12.014.
  44. G. Franceschi, M. Schmid, U. Diebold and M. Riva, Atomically resolved surface phases of La0.8Sr0.2MnO3(110) thin films, J. Mater. Chem. A, 2020, 8, 22947–22961,  10.1039/d0ta07032g.
  45. A. N. Grundy, B. Hallstedt and L. J. Gauckler, Assessment of the La–Sr–Mn–O system, Calphad, 2004, 28, 191–201,  DOI:10.1016/j.calphad.2004.07.001.
  46. G. Franceschi, M. Wagner, J. Hofinger, T. Krajňák, M. Schmid, U. Diebold and M. Riva, Growth of In2O3(111) thin films with optimized surfaces, Phys. Rev. Mater., 2019, 3, 1–10,  DOI:10.1103/PhysRevMaterials.3.103403.
  47. S. Wicklein, A. Sambri, S. Amoruso, X. Wang, R. Bruzzese, A. Koehl and R. Dittmann, Pulsed laser ablation of complex oxides: The role of congruent ablation and preferential scattering for the film stoichiometry, Appl. Phys. Lett., 2012, 101, 13601,  DOI:10.1063/1.4754112.
  48. S. Amoruso, C. Aruta, R. Bruzzese, D. Maccariello, L. Maritato, F. M. Granozio, P. Orgiani, U. di Uccio and X. Wang, Optimization of La0.7Ba0.3MnO3−δ complex oxide laser ablation conditions by plume imaging and optical emission spectroscopy, J. Appl. Phys., 2010, 108, 43302,  DOI:10.1063/1.3467770.
  49. P. Orgiani, R. Ciancio, A. Galdi, S. Amoruso and L. Maritato, Physical properties of La0.7Ba0.3MnO3−δ complex oxide thin films grown by pulsed laser deposition technique, Appl. Phys. Lett., 2010, 96, 32501,  DOI:10.1063/1.3292588.
  50. M. Tyunina, J. Levoska and S. Leppävuori, Experimental studies and modeling of Pb-Zr-Ti-O film growth in pulsed laser deposition, J. Appl. Phys., 1998, 83, 5489–5496,  DOI:10.1063/1.367379.
  51. G. Z. Liu, Q. Y. Lei and X. X. Xi, Stoichiometry of SrTiO3 films grown by pulsed laser deposition, Appl. Phys. Lett., 2012, 100, 202902,  DOI:10.1063/1.4717984.
  52. T. Ohnishi, K. Shibuya, T. Yamamoto and M. Lippmaa, Defects and transport in complex oxide thin films, J. Appl. Phys., 2008, 103, 103703,  DOI:10.1063/1.2921972.
  53. B. Dam, J. H. Rector, J. Johansson, J. Huijbregtse and D. G. De Groot, Mechanism of incongruent ablation of SrTiO3, J. Appl. Phys., 1998, 83, 3386–3389,  DOI:10.1063/1.367106.
  54. J. A. Enterkin, A. K. Subramanian, B. C. Russell, M. R. Castell, K. R. Poeppelmeier and L. D. Marks, A homologous series of structures on the surface of SrTiO3(110), Nat. Mater., 2010, 9, 245,  DOI:10.1038/nmat2636.
  55. G. Franceschi, M. Schmid, U. Diebold and M. Riva, Reconstruction changes drive surface diffusion and determine the flatness of oxide surfaces, J. Vac. Sci. Technol., A, 2022, 40, 023206,  DOI:10.1116/6.0001704.
  56. M. Brahlek, A. Sen Gupta, J. Lapano, J. Roth, H. T. Zhang, L. Zhang, R. Haislmaier and R. Engel-Herbert, Frontiers in the growth of complex oxide thin films: past, present, and future of hybrid MBE, Adv. Funct. Mater., 2018, 28, 1702772,  DOI:10.1002/adfm.201702772.
  57. K. Rachut, T. J. M. Bayer, J. O. Wolff, B. Kmet, A. Benčan and A. Klein, Off-stoichiometry of magnetron sputtered Ba1−xSrxTiO3 thin films, Phys. Status Solidi B, 2019, 256, 1970039,  DOI:10.1002/pssb.201970039.
  58. S. Gerhold, M. Riva, B. Yildiz, M. Schmid and U. Diebold, Adjusting island density and morphology of the SrTiO3(110)-(4×1) surface: Pulsed laser deposition combined with scanning tunneling microscopy, Surf. Sci., 2016, 651, 76,  DOI:10.1016/j.susc.2016.03.010.
  59. D. Kriegner, E. Wintersberger and J. Stangl, xrayutilities: A versatile tool for reciprocal space conversion of scattering data recorded with linear and area detectors, J. Appl. Crystallogr., 2013, 46, 1162,  DOI:10.1107/S0021889813017214.
  60. D. S. Mebane, Y. Liu and M. Liu, Refinement of the bulk defect model for LaxSr1−xMnOδ, Solid State Ionics, 2008, 178, 1950,  DOI:10.1016/j.ssi.2008.01.016.
  61. C. Dong, F. Wu and H. Chen, Correction of zero shift in powder diffraction patterns using the reflection-pair method, J. Appl. Crystallogr., 1999, 32, 850,  DOI:10.1107/S0021889899007396.
  62. H. D. Megaw and C. N. W. Darlington, Geometrical and structural relations in the rhombohedral perovskites, Acta Crystallogr., Sect. A: Cryst. Phys., Diffr., Theor. Gen. Crystallogr., 1975, 31, 161,  DOI:10.1107/S0567739475000332.
  63. T. Darling, A. Migliori, E. Moshopoulou, S. A. Trugman, J. Neumeier, J. Sarrao, A. Bishop and J. Thompson, Measurement of the elastic tensor of a single crystal of La0.83Sr0.17MnO3 and its response to magnetic fields, Phys. Rev. B: Condens. Matter Mater. Phys., 1998, 57, 5093,  DOI:10.1103/PhysRevB.57.5093.
  64. P. M. Marcus and F. Jona, Strains in epitaxial films: The general case, Phys. Rev. B: Condens. Matter Mater. Phys., 1995, 51, 5263,  DOI:10.1103/PhysRevB.51.5263.
  65. P. Virtanen, R. Gommers, T. E. Oliphant, M. Haberland, T. Reddy, D. Cournapeau, E. Burovski, P. Peterson, W. Weckesser, J. Bright, S. J. van der Walt, M. Brett, J. Wilson, K. J. Millman, N. Mayorov, A. R. J. Nelson, E. Jones, R. Kern, E. Larson, C. J. Carey, İ. Polat, Y. Feng, E. W. Moore, J. VanderPlas, D. Laxalde, J. Perktold, R. Cimrman, I. Henriksen, E. A. Quintero, C. R. Harris, A. M. Archibald, A. H. Ribeiro, F. Pedregosa, P. van Mulbregt and SciPy 1.0 Contributors, SciPy 1.0: fundamental algorithms for scientific computing in Python, Nat. Methods, 2020, 17, 261,  DOI:10.1038/s41592-019-0686-2.
  66. S. Gražulis, D. Chateigner, R. T. Downs, A. F. T. Yokochi, M. Quirós, L. Lutterotti, E. Manakova, J. Butkus, P. Moeck and A. Le Bail, Crystallography Open Database – An open-access collection of crystal structures, J. Appl. Crystallogr., 2009, 42, 726,  DOI:10.1107/S0021889809016690.

Footnote

Electronic supplementary information (ESI) available: S1: Materials and methods; S2: RBS and XRD characterization of atomically flat films; S3: UHV strategies to recover ideal morphologies. See DOI: https://doi.org/10.1039/d3na00847a

This journal is © The Royal Society of Chemistry 2023