Open Access Article
Muhammad Ali
Ehsan
a,
Abuzar
Khan
*a,
Munzir H.
Suliman
a and
Mohamed
Javid
b
aInterdisciplinary Research Center for Hydrogen and Energy Storage (IRC-HES), Saudi Arabia. E-mail: abuzar@kfupm.edu.sa
bCore Research Facilities, King Fahd University of Petroleum & Minerals, Box 5040, Dhahran 31261, Saudi Arabia
First published on 4th September 2023
Bimetallic iron-nickel (FeNi) compounds are widely studied materials for the oxygen evolution reaction (OER) owing to their high electrocatalytic performance and low cost. In this work, we produced thin films of the FeNi alloy on nickel foam (NF) by using an aerosol-assisted chemical deposition (AACVD) method and examined their OER catalytic activity. The hybrid FeNi/Ni catalysts obtained after 1 and 2 h of AACVD deposition show improved charge transfer and kinetics for the OER due to the strong interface between the FeNi alloy and Ni support. The FeNi/Ni-2h catalyst has higher catalytic activity than the FeNi/Ni-1h catalyst because of its nanoflower morphology that provides a large surface area and numerous active sites for the OER. Therefore, the FeNi/Ni-2h catalyst exhibits low overpotentials of 300 and 340 mV at 50 and 500 mA cm−2 respectively, and excellent stability over 100 h, and ∼0% loss after 5000 cycles in 1 M KOH electrolyte. Furthermore, this catalyst has a small Tafel slope, low charge transfer resistance and high current exchange density and thus surpasses the benchmark IrO2 catalyst. The easy, simple, and scalable AACVD method is an effective way to develop thin film electrocatalysts with high activity and stability.
The incompletely filled ‘d’ orbital of Ni allows easy transfer of electrons and hence its alloys are expected to have high catalytic activity and potential for large-scale applications.21 Nickel alloys with noble metals have been widely investigated due to their outstanding activity and stability as efficient electrocatalysts for water electrolysis.22 Currently, research is focused on developing Ni alloy electrocatalysts with other non-noble metals such as Mo, Cr, Fe, etc.23–25 Alloys of Ni and Fe are reported as the most promising electrocatalysts for oxygen evolution reactions due to their low cost, high activity, and stability.23 Ni and Fe-based OER materials, including oxides, hydroxides, layered hydroxides, and alloys of binary and tertiary metal composites have been reported recently in several OER studies.26–29 Notably, E. Hatami et al.30 reported a novel Ni–Fe micro/nano urchin-like structure fabricated by a fast and one-step electrodeposition strategy which required overpotentials of only 292 and 374 mV to deliver 10 and 100 mA cm−2. In another study,31 a variant of the Fe–Ni catalyst developed on the carbon cloth support delivered a low overpotential of 290 mV with a Tafel slope of 51 mV dec−1 at a current density of 10 mA cm−2. Similarly, various nickel–iron combinations have shown promising results for OER catalysis.32,33 These studies have indicated that the catalyst fabrication process, morphology and support material are the important parameters which contribute towards higher efficiency of the OER. It has been observed that previous OER studies based on the NiFe electrocatalyst used nano powders, which certainly require some polymer binders (like Nafion) for better adhesion with the current collector. The addition of binder covers the active sites of the catalyst and causes its deactivation. Meanwhile, it increases the resistance between the catalyst and the current collector and hinders the easy transfer of electrons, thereby deteriorating the conductivity. Moreover, such bonded catalysts are not mechanically stable, and the catalyst easily flakes off under severe oxygen evolution conditions, particularly when higher current densities are applied.34 These issues need to be solved to understand the full potential of nanostructured catalysts. Therefore, by developing a polymeric binder-less electrocatalytic thin film, higher conductivity can be achieved, resulting in improved electrocatalytic activity.
In the current work, we have developed an iron-nickel (FeNi) alloy catalyst directly on nickel foam (NF) by following a thin film deposition process based on aerosol assisted chemical vapor deposition (AACVD). AACVD is a custom designed, inexpensive, and single step thin film fabrication process which can create nanomaterials directly on a support surface without any need of binder or reagent to bind the catalyst with the support. As the catalyst is directly developed over the support surface, the inherent conductivity of the catalyst is retained. Moreover, the nano morphologies can be easily controlled with the deposition parameters such as deposition time, temperature, and nature of solvent. Thus, porous Fe–Ni thin alloy film catalysts produced on nickel foam for time periods of 1 h and 2 h have been investigated for the OER. The FeNi catalyst grown for 2 h initiated water oxidation at 1.4 V vs. RHE (=170 mV) and achieved current densities of 50 and 500 mA cm−2 by consuming overpotentials of 300 and 340 mV respectively. Moreover, the catalyst remained stable for over 100 h under the continuous water oxidation operation performed at varying current densities. The catalyst outperformed the benchmark IrO2/NF catalyst when tested for the OER under similar conditions. The competitive activity and outstanding durability of the FeNi/Ni alloy catalyst demonstrate its great ability to replace precious metal catalysts in future practical applications.
The iron–nickel alloy (FeNi) thin film electrocatalyst was developed on Ni foam using an in-house built aerosol-assisted chemical vapor deposition (AACVD) strategy. The schematic presentation of AACVD and its operational details have been described in our earlier work. The solution of the dual precursor of Fe(acac)3 (100 mg, 0.283 mmol) and Ni(acac)2 (73 mg, 0.283 mmol) was prepared in 15 mL of methanol. The aerosol mist from the dual precursor solution was produced using an ultrasonic humidifier, and a mist stream was transferred to a horizontal tube furnace preheated at 475 °C with the help of carrier gas (10% H2 + 90% N2). The NF in the tube furnace was positioned to receive the precursor nebula directly over it, where the decomposition of the precursor and CVD reactions took place to develop a layer of FeNi material. The deposition process was repeated for a period of 1 h and 2 h, respectively and the prepared samples were named as FeNi/Ni-1h and FeNi/Ni-2h, respectively. After completing the deposition experiments, the aerosol supply was closed and 100% H2 gas was passed over the catalyst films to ensure the FeNi alloy formation. The amount of the deposited FeNi alloy on NF was obtained from the difference in the weight of NF before and after deposition. The amount of the FeNi alloy on FeNi/Ni-1h and FeNi/Ni-2h was found to be 47 μg and 88 μg respectively.
V′ = iR; where V′ is the iR-corrected potential, and i is the value of current obtained from the CV and LSV measurements. Rs is the value of solution resistance obtained from the EIS measurement after electrochemical fitting. The solution resistance was determined by fitting the high-frequency region of the EIS data with an equivalent circuit. The iR correction was performed after the CV and LSV measurements were completed. The iR-corrected data were then used for further analysis.
![]() | ||
| Fig. 1 XRD patterns of iron-nickel (Fe–Ni) alloy films grown on plain glass for periods of 1 and 2 h via AACVD. | ||
Fig. 2 shows the SEM morphology of the FeNi alloy catalyst produced on nickel foam as a result of 1 and 2 h deposition via AACVD. The FeNi/Ni-1h alloy shows the formation and distribution of small sized crystallites over a large area of NF struts (Fig. 2a). The design, shape and texture of these crystallites become visible in a high-magnification image, which exhibits a blooming flower-like pattern with regularly interconnected petal features. The direct deposition for 2 h developed a significantly large and thick plant-like object and its corresponding high-magnification image clearly shows the vertically aligned petals which are stacked together to create another flower pattern. The development of hierarchical flower like structures in both catalyst samples seems fluffy and porous presenting a high surface area with uniform distribution of catalytically active sites. The 3D NF with hierarchical and porous petal networks offers a promising platform for various applications such as water splitting, supercapacitors, and hydrogen storage.25,36–38 The petal networks facilitate the contact between the electrolyte ions and the catalyst material. The FeNi petals synthesized after 2 h of deposition time have more active centers at the surface that can enhance the OER performance. These active centers are influenced by the surface structure, nanoparticle shape/size and the electrolyte composition.
The elemental composition of the FeNi alloy catalyst was investigated by EDX analysis. For this, the catalyst film prepared on a plain glass was used to avoid the addition of Ni from the nickel foam substrate, which might otherwise increase the concentration of Ni present in the as-synthesized catalyst samples. The presence of Fe and Ni elements suggests the synthesis of FeNi catalysts, and the Au peaks are attributed to the gold coating used to avoid the charging effect under SEM. The percent (%) atomicity in the FeNi alloy catalyst is found to be 47.6/52.4 and 48.3/51.7 representing an empirical elemental ratio between Fe
:
Ni atoms, which is nearly 1 to 1. The absence of the oxygen (O) element indicates the synthesis of the pure alloy material. Additionally, the EDX map analysis (Fig. S1†) confirmed that Fe and Ni atoms are homogenously and uniformly distributed in the alloy materials.
The nanostructure of the FeNi/Ni-2h catalyst was further analyzed by TEM analysis (Fig. 3). The nano-sheet like morphology found in TEM images (Fig. 3a and b) indicates a good correlation with the SEM result. The TEM images show the presence of quantum dots of size 2–4 nm inside these nanosheets. Although it is hard to identify Fe and Ni atoms, the value of the characteristic spacing is 0.20 nm,39 corresponding well to the high intensity (111) crystal facet of metallic nickel as observed in XRD data. Furthermore, the selected area electron diffraction pattern (SAED) (Fig. 3d) shows the formation of symmetrical rings demonstrating the poly-crystalline nature of the FeNi alloy catalyst.
After surface activation and stabilization of the fabricated electrocatalysts, their OER performance was evaluated and compared using linear sweep voltammetry (LSV) performed in 1.0 M KOH solution at a scan rate of 5 mVs−1. For comparison, bare NF and IrO2 coated NF were also tested under similar conditions. Fig. 4a shows the polarization curves of all catalytic systems. Apparently, in all catalytic systems, the current density peak rapidly increases after 1.5 V. The comparative LSV curves clearly show that both FeNi/Ni-1h and FeNi/Ni-2h have better OER performance when compared with IrO2/NF and bare NF. Particularly, FeNi/Ni-2h reaches a maximum current density of 700 mA cm−2 at 1.57 V, while FeNi/Ni-1h only reaches a current density of 500 mA cm−2 at a higher potential of 1.65 V, indicating a faster heterogeneous electron transfer process in the FeNi/Ni-2h catalyst. The benchmark IrO2 and bare nickel foam exhibit higher potentials and lower peak current densities compared to both FeNi catalysts. Fig. 4b presents the enlarged view of these LSV curves, which clearly show that water oxidation in the FeNi/Ni-2h catalyst begins a bit earlier (at 1.47 V ηonset = 240 mV) than that in the FeNi/Ni-1h catalyst (1.53 V ηonset = 300 mV), while both catalysts maintained a potential difference (Δη) of 40 mV to reach a current density of 50 mA cm−2. Nevertheless, to reach a current density of 50 mA cm−2, the FeNi/Ni-1h catalyst requires an overpotential of 340 mV which is less than that of the benchmark IrO2 (370 mA).
Further, the Tafel slope has been extracted from the polarization curves to compare the OER kinetics of different catalysts involved in this study. The Tafel equation: η = a + b
log
j is used to fit the linear part of the Tafel curve and Fig. 4c shows that FeNi/Ni-2h has the lowest Tafel slope value of 39 mV dec−1 followed by FeNi/Ni-1h (69 mV dec−1) IrO2 (95 mV dec−1) and bare NF (195 mV dec−1). The smaller Tafel value of the FeNi/Ni-2h catalyst indicates its ability to transfer charge at faster rates than the other catalysts, and thus it shows superior OER activity to FeNi alloy catalysts indicating a higher OER kinetics on the FeNi surface.
A further insight into electrocatalyst kinetics is obtained through electrochemical impedance spectroscopy (EIS) which describes about the electrical resistance and interfacial charge transfer resistance (Rct) between the surface of an electrode and H2O/OH. The electrical conductivity of an electrode is a crucial factor that modifies its efficacy. Typically, higher electrical conductivity results in a quicker charge transfer and consequently greater performance. Fig. 4d depicts the EIS Nyquist plots of all electrocatalysts (NF, IrO2, FeNi/Ni-1h, and FeNi/Ni-2h) recorded at a potential of 1.5 VRHE. The resistance or kinetics of interfacial charge transfer near the electrode surface can be inferred from the semicircular dispersion in Nyquist plots. The semicircular arcs represent the frequency response of the transfer function in Cartesian coordinates. The smaller the arc, the lower the resistance or faster the charge transfer. A two-time constant parallel model was used to fit all EIS data, based on the Nyquist analysis that showed the existence of a circuit with two-time constants. This model consists of Rs in series with two parallel constant phase element-resistance. The Rs represents collective resistances, including wiring resistance (Rwiring) and solution resistance (Rsolu). In addition, Rct and Rp represent, respectively,42,43 (summarized in Table 1) the charge transfer resistance and surface (porous or irregular texture) resistance. The FeNi/Ni-2h catalyst demonstrates the lowest Rct value and hence better charge transport and conductivity as compared to the other electrocatalysts.
| Electrocatalyst | R s | R p | R ct |
|---|---|---|---|
| NF | 2.1 | 22.2 | 2.10 × 104 |
| IrO2 | 1.9 | 0.11 | 51 |
| FeNi/Ni-1h | 0.85 | 0.1 | 11.4 |
| FeNi/Ni-2h | 1 | 1.8 | 2.8 |
In addition, the inherent catalytic activity of both FeNi electrocatalysts was assessed by measuring the turnover frequency (TOF) using the following formula:
485 C mol−1, and m is the number of moles of catalyst that have been deposited on the NF substrate.42,44Fig. 4e indicates the TOF plot of the FeNi electrocatalysts measured at various overpotentials. The FeNi/Ni-1h and FeNi/Ni-2h electrocatalysts exhibit TOF values of 0.25 s−1 and 1.85 s−1, respectively at an overpotential of 350 mV. The FeNi/Ni-2h electrode has a significantly larger TOF value than its analog (NiFe-1h), which reveals its highly conducting nature and superior OER activity. The intrinsic electrocatalytic activity was further evaluated by studying the exchange current density (J0). The exchange current density reflects the electron transfer ability of the catalyst material. Electrocatalysts with higher current density need less driving force to drive the charges. The exchange current density is obtained by extending the linear part of the Tafel curve to the X-axis (Fig. 4f). At zero over potential, the log
[j] values of FeNi/Ni-1h and FeNi/Ni-2h are found to be 0.044 and 0.65 which correspond to the J0 values of 2.7 and 4.4 mA cm−2, respectively. Again, the higher exchange current density of the FeNi/Ni-2h catalyst makes it remarkable for OER catalysis.
Besides higher electrocatalytic activity, long term OER stability is another important factor which decides the suitability of a catalyst for practical demonstration. The FeNi/Ni-2h catalyst was subjected to prolonged OER measurements by two different kinds of tests. First, the catalyst was subjected to a continuous CV run for 5000 cycles and the results of the 1st and 5000th cycles are compared in Fig. 5a which have the same profile. After CV, the chronopotentiometric (CP) test for more than 100 h was carried out by applying two potentials of 1.50 and 1.52 V, respectively to observe the corresponding current profiles displayed in Fig. 5b, which shows a linear behavior. Both stability tests (CV and CP) show the high stability and endurance of the FeNi electrocatalyst under rigorous OER conditions. Right after CP measurement, the polarization curve was measured again and compared with its response before the stability test as shown in Fig. 5c. The polarization curve after the stability test is consistent with its initial behavior.
In order to investigate the compositional change in the FeNi/Ni-2h catalyst as a result of 100 h of chronopotentiometric testing, EDX analysis was conducted. Fig. S3† indicates the EDX spectrum which reveals the presence of mandatory Fe and Ni atoms on the surface of the catalyst. However, the concentration of oxygen, which was completely absent before the OER (Fig. S1†), has significantly increased after long term OER. The presence of oxygen suggests the formation of NiFeOx due to the occurrence of oxidation reaction.
The influential OER performance of the FeNi alloy thin film electrocatalyst can be attributed to the following factors: (i) the use of a suitable deposition method based on AACVD to develop FeNi thin films directly on the nickel foam support resulted in a robust electrocatalyst which enhanced the electrical conductivity of the catalyst, (ii) the 2 h deposition yielded a highly porous nanoflower structure providing abundantly available catalytically active sites to facilitate improved reaction kinetics, and (iii) the porosity and 3-D texture of Ni-foam as a support allow penetration, increase electron/ion transport paths, and excessively disperse the electroactive phase.
Finally, Table 2 compares the key water oxidation parameters of different types of bimetallic Fe–Ni electrocatalysts prepared by different methods on different substrates. The FeNi alloy film catalyst prepared for 2 h by the AACVD process clearly shows a lower overpotential and has a tendency to produce a higher current density of <700 mA cm−2 as compared to the other electrocatalysts.
| Catalyst/system | Support | Synthetic strategy | Potential [mV] @ 50 mA cm−2 | Peak current density [mA cm−2] | Tafel slope [mV dec−1] | Ref. |
|---|---|---|---|---|---|---|
| FeNi-2h | NF | AACVD | 300 | <700 | 39 | This work |
| Ni–Fe–P | NF | Electrodeposition | 330 | ∼140 | 69 | 45 |
| Fe0.4Ni0.6 alloy | NF | Heat treatment process | 300 | 120 | 67 | 46 |
| Fe–Ni–Ox NPs | NF | Aerosol spray approach | 315 | >80 | 38 | 47 |
| Ni–Fe alloy | Cu foil | Electrodeposition | 325 | 350 | 86 | 30 |
| (Ni0.5Fe0.5)2P | GC | Ketjenblack carbon (KB)-templated | ∼380 | 120 | 77 | 48 |
| NiFeOOH | GC | Electrodeposition | 375 | 50 | NA | 49 |
| Metallic Ni thin film | NF | AACVD | 310 | >700 | 73 | 44 |
| IrO2 | Glassy carbon | Commercial | 301 | >170 | 75 | 50 |
| RuO2 | NF | Commercial | 322 | 400 | 55 | 51 |
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3na00298e |
| This journal is © The Royal Society of Chemistry 2023 |