Open Access Article
S.
Swathi
a,
R.
Yuvakkumar
*a,
G.
Ravi
a,
Abdullah G.
Al-Sehemi
bc and
Dhayalan
Velauthapillai
*d
aDepartment of Physics, Alagappa University, Karaikudi 630 003, Tamil Nadu, India. E-mail: yuvakkumarr@alagappauniversity.ac.in
bResearch Centre for Advanced Materials Science, King Khalid University, Abha 61413, Saudi Arabia
cDepartment of Chemistry, King Khalid University, Abha 61413, Saudi Arabia
dFaculty of Engineering and Science, Western Norway University of Applied Sciences, Bergen 5063, Norway. E-mail: dhayalan.Velauthapillai@hvl.no
First published on 18th May 2022
In the present work, samarium-doped nickel manganese oxide was produced by employing a straightforward co-precipitation method. A peak with a 2θ of 36° corresponded to the (110) plane confirming the formation of the rhombohedral crystal structure of NiMnO3. The existence of Mn–O and Ni–O stretching vibration modes was confirmed by Raman spectroscopy. FTIR spectra confirmed the existence of the metal–oxygen bond of NiMnO3. The synthesized ternary Ni-based material was found to be spherical nanoparticles with an average diameter of 0.81 μm. The electrochemical oxygen evolution reaction (OER) performance was explored on 0.02 M samarium (Sm)-doped NiMnO3 demonstrating outstanding OER action with low 321 mV, a low Tafel slope value (109 mV dec−1), and low charge-transfer resistance (0.19 Ω). Moreover, the BET results suggest that the 0.02 M Sm-doped NiMnO3 exhibited elevated surface area (78.78 m2 g−1) with a mesoporous character. Therefore, NiMnO3 doped with high concentrations of a rare earth metal, Sm, is proposed as a suitable material for next-generation water splitting applications.
Transition metal oxides are promising materials for various applications, such as for use in lithium-ion batteries, supercapacitors, water oxidation, hydrogen production, and urea oxidation.6 However, they have limited application due to their poor conductivity and insufficient active sites. Attempts have been made to overcome these issues by various approaches, such as the incorporation of metal ions, the introduction of carbon-based materials and quantum dots, etc.7 In particular, rare earth metal-doped metal oxides exhibit excellent activities, which improve the conductivity of the material and the surface area, and enhance the diffusion paths.8 Numerous rare-earth metals, such as gadolinium, neodymium, dysprosium, and samarium have been used as doping agents.9 Among these metals, samarium dramatically improves the ionic conductivity, carrier transportability, and catalytic performance.10 In addition, nickel-based materials have gained special attention for the oxygen evolution reactions (OER) due to their benefits of lower water oxidation potential.11 Many methods are now available to prepare metal oxide electrocatalysts via hydrothermal, co-precipitation and microwave-assisted techniques, etc.12 Amongst these, co-precipitation is a less time-consuming technique performed at low temperatures.13
Numerous researchers have assessed the application of nickel manganese oxide (NMO) for various purposes. For example, Mustafa Al Samarai et al.14 synthesized a graphene-supported Ni3MnO4 catalyst by a reverse micellar method for electrocatalytic OER. Yan Zhang et al.15 synthesized a nickel manganese composite oxide nanomesh via the hydrothermal method, followed by high-temperature calcination for use in supercapacitors and electrochemical water oxidation. Dongxiao Ji et al.16 fabricated carbon-based nickel and manganese oxide nanoparticles via the electrospinning-calcination method for electrochemical water oxidation. In this study, NMO was synthesized from the co-precipitation and subsequent calcinations for the OER. Structural and morphological studies confirmed the formation of NiMnO3 nanocomposite. In addition, the doping agent, samarium, not only changed the electrical properties of the nanocomposite but also improved the electrochemical performance of the nanocomposite material.
:
1) molar ratio of nickel and manganese precursors was mixed and dissolved with 50 ml of deionized water. After stirring well, 1.0 M sodium bicarbonate was added; within some hours, a green-bluish precipitate appeared, which was washed with distilled water, ethanol, and methanol. The material thus obtained was transferred to the oven at 80 °C for 12 h. After drying, the product was annealed at 400 °C for 4 h. The formation of a black fine powder indicated the formation of NMO. Likewise, different concentrations of samarium (0.01 and 0.02 M)-doped NMO samples were synthesized by the above procedure using appropriate ratios of materials. The black powder samples were labeled NMO1, NMO2, and NMO3. The electrochemical water oxidation analysis of the synthesized products was examined in three electrode workstations. In these workstations, platinum was used as a counter electrode, Ag/AgCl was used as a reference electrode. The NMO samples were employed as working electrodes with 1 M KOH as the electrolyte.
![]() | ||
| Fig. 1 (A) XRD spectra (B) Raman, and (C) FTIR spectra of pristine NiMnO3, 0.01 M Sm-doped NiMnO3, and 0.02 M Sm-doped NiMnO3. | ||
Fig. 2(A–F) shows the SEM images of pure NiMnO3 and different concentrations (0.01, 0.02 M) of Sm-doped NiMnO3, suggesting the particles to be in the micro range in size between 10 and 5 μm. The images revealed that the particles have a spherical shape with diameters of 2.26 μm (pure NiMnO3), 2.0 μm (0.01 M Sm-doped NiMnO3), and 0.81 μm (0.02 M Sm-doped NiMnO3). These sizes were calculated using the Image J software. In a zoomed-in view, fine nanoparticles were seen to co-exist (Fig. 2B, D and F). Moreover, it was observable that the particle size of NiMnO3 decreased from 2.26 to 0.81 μm, when the content of Sm dopant increased from 0 to 0.02 M. The agglomeration was also slightly reduced because of doping. In addition, the average particle sizes may decrease with increasing Sm concentrations, due to the existence of smaller radii. In detail, the ionic radius of Sm3+ was 1.08 Å and Ni3+ was 70 Å. Therefore, the radius of Sm3+ was very small as compared to that of Ni3+. Furthermore, smaller average particle sizes may be attributed due to inhibited grain growth due to the substituted Sm ions at the Ni sites. The reduced particle sizes significantly promoted the edge and corner-site contact at the catalyst surface, which enabled the formation of reaction intermediates, accelerated catalytic kinetics, and enhanced electrochemical water oxidation.20,21 Overall, SEM analysis suggested that increased dopant concentrations decreased the particle size, denoting that the synthesized product developed a more crystalline nature.22
![]() | ||
| Fig. 2 SEM images (A and B) pristine NiMnO3, (C and D) 0.01 M Sm-doped NiMnO3, and (E and F) 0.02 M Sm-doped NiMnO3 at 10 and 5 μm. | ||
The incorporation of the doping agent, Sm, was confirmed by the EDX spectra as shown in Fig. 3. The synthesized material comprised 23.68% Ni, 32.40% Mn, 28.45% O, and 15.47% Sm by weight percentage. Moreover, the sample contained 14.03% Ni, 20.52% Mn, 61.87% O, and 3.58% Sm by atomic percentage. No other elements representing impurities were observed.
Fig. 4 shows the results of the BET surface area analysis of pure, 0.01 M, and 0.02 M Sm-doped NiMnO3. According to the BET studies, the surface area, pore-volume, and diameter of pure, 0.01 M, and 0.02 M Sm-doped NiMnO3 were found and are presented in Table 1. Results revealed that 0.02 M Sm-doped NiMnO3 had a higher surface area than other materials. Moreover, the obtained graphs depict a type IV isotherm with discrete H4 hysteresis, proving the mesoporous nature of the synthesized material. The high surface area and porous properties of the 0.02 M Sm-doped NiMnO3 can reduce diffusion lengths, facilitating the penetration of electrolyte ions and improving the transport pathway in the electrochemical analysis.23 Moreover, the elevated surface area offers additional active sites and helps improve electrochemical OER performance.
![]() | ||
| Fig. 4 (A) Nitrogen adsorption–desorption and (B) BJH pore diameter of pristine NiMnO3, 0.01 M Sm-doped NiMnO3, and 0.02 M Sm-doped NiMnO3. | ||
| Materials | Surface area | Pore volume | Pore diameter |
|---|---|---|---|
| NiMnO3 | 38.065 m2 g−1 | 0.174 cc g−1 | 1.960 nm |
| 0.01 M Sm–NiMnO3 | 44.332 m2 g−1 | 0.176 cc g−1 | 14.857 nm |
| 0.02 M Sm–NiMnO3 | 78.78 m2 g−1 | 0.439 cc g−1 | 11.252 nm |
The LSV curves of pure, 0.01 M, and 0.02 M Sm-doped NiMnO3 were recorded from 0 to 1 V at 2 mV s−1 (Fig. 5A). The 0.02 M Sm-doped NiMnO3 showed better OER activity and required only 321 mV to reach the benchmark of 10 mA cm−2. Contrarily, the other electrocatalysts, such as pristine NiMnO3 and 0.01 M Sm-doped NiMnO3, need 371 and 335 mV to attain the same current density (Fig. 5C). Generally, Ni-based binary or ternary materials exhibit excellent electrochemical performance than pure Ni materials.24 Moreover, the rare earth dopant, Sm, also improved the surface area, further improving the OER activity. The electrode material had a larger surface area as compared to the electrocatalyst. Hence, superior electrochemical performance was expected due to the addition of Sm to NiMnO3, which could, in turn, produce high electrochemical OER activity. A comparison of these findings with those from previous literature is tabulated in Table 2.
![]() | ||
| Fig. 5 (A) LSV spectra, (B) Tafel slope (C) Bar diagram (inset: error bar), and (D) EIS spectra of pristine NiMnO3, 0.01 M Sm-doped NiMnO3, and 0.02 M Sm-doped NiMnO3. | ||
| Material | Overpotential values | Tafel slope values | Ref. |
|---|---|---|---|
| NiO | 396 mV | 54 mV dec−1 | 25 |
| NiFe2O4 hollow fiber/Ni foam | 433 mV | 134 mV dec−1 | 26 |
| 3D NiOx/Ni foam | 390 mV | 80 mV dec−1 | 27 |
| NiO hollow nanofibers/Ni foam | 340 mV | 84 mV dec−1 | 28 |
| Ni0.9Fe0.1Ox | 340 mV | 31 mV dec−1 | 29 |
| MnO2 NSs | 423 mV | 79.6 mV dec−1 | 30 |
| MnO2 NSs/Co3O4 NPs-1:2 | 355 mV | 56.5 mV dec−1 | 30 |
| Sm-NiMnO3 | 321 mV | 109 mV dec−1 | [Present work] |
Tafel slope curves were derived from the polarization curves, which were then used to investigate the material OER kinetics (Fig. 5B). Tafel slopes of 138, 136, and 109 mV/dec were obtained for pure NiMnO3, 0.01 M, and 0.02 M Sm-doped NiMnO3. 0.02 M Sm-doped NiMnO3 showed a small slope of 109 mV/dec as compared to the other two materials. A low Tafel slope value denotes rapid electron transport and superb OER catalytic kinetics.31
The EIS analysis was performed on all prepared materials, to obtain further information on OER kinetics (Fig. 5D). 0.02 M Sm-doped NiMnO3 presented charge transfer (Rct) and solution resistance (Rs) of 0.19 and 0.76 Ω, respectively, which were smaller than those of other materials, i.e., 0.01 M Sm doped NiMnO3 (Rs = 0.77 Ω, Rct = 0.20 Ω) and pure NiMnO3 (Rs = 0.96 Ω, Rct = 0.26 Ω). The fitted equivalent circuit has been inserted in Fig. 5D. These results suggest that the 0.02 M Sm-doped NiMnO3 had more favorable OER kinetics because a low Rct value denotes highly proficient charge transfer and a speedier faradaic process.32
The electrochemical activity towards OER was further studied with the help of double-layer capacitance. The cyclic voltammogram was obtained at a potential of 0.26–0.34 V at various scan rates of 20, 40, 80, and 100 mV s−1, respectively (Fig. 6(A–C)). As predicted, 0.02 M Sm-doped NiMnO3 showed Cdl values of 25.2 mF cm−2, whereas the 0.01 M Sm-doped NiMnO3 and pure NiMnO3 showed the Cdl values of 8.3 and 4.1 mF cm−2, respectively (Fig. 5D). Moreover, the electrochemical active surface area (ECSA) was estimated following the equation: ECSA = Cdl/Cs; Cdl - double-layer capacitance and Cs - sample-specific capacitance. The estimated ECSA of pure NiMnO3, 0.01 M, and 0.02 M-Sm doped NiMnO3 were 0.205, 0.415, and 1.26 cm2 respectively. These results suggest that the incorporation of Sm in NiMnO3 provided greater surface area, which could offer additional exposed surface reactive sites for OER activity.33
![]() | ||
| Fig. 6 (A–C) CV Curves and (D) double-layer capacitance for pristine NiMnO3, 0.01 M, 0.02 M Sm-doped NiMnO3, chronoamperometry test of 0.02 M Sm-doped NiMnO3 for (E) 2 h and (F) 16 h. | ||
A durability test for 0.02 M Sm-doped NiMnO3 was performed using chronoamperometry (Fig. 6E and F). No further changes were observed in the current density of 0.02 M Sm-doped NiMnO3 with 98.5% retention after 2 h (Fig. 6E). Moreover, the same electrode was tested again for 16 h, whereby it exhibited 97.6% retention, clearly suggesting the material's stability in prolonged hours (Fig. 6F). Overall, the results suggest that the introduction of Sm to NiMnO3 imparts excellent OER activity and stability to NiMnO3 owing to the higher surface area, electrical conductivity, and abundance of catalytic active sites in the Sm-doped material.34
| This journal is © The Royal Society of Chemistry 2022 |