Recently, CsPbX3 (X = I, Br, Cl) nanocrystals (NCs) have shown huge potential in the fields of various optoelectronic applications. However, the CsPbX3 NCs degrade very rapidly in the presence of water and heat, because of dynamic oleic acid and oleylamine capping ligands. The silica-coated CsPbBr3 NCs are comparatively stable but the synthesis is slightly complicated and needs several hours to complete the reaction process. These silica-coated NCs also tend to agglomerate among themselves, which is unfavorable for display technologies and bioimaging applications. In these regards, we introduce novel polymers [polyvinylpyrrolidone and n-isopropyl acrylamide] along with oleic acid and oleylamine that are encapsulated around the CsPbBr3 NCs during the synthesis procedure at room temperature. Such NCs are highly luminescent in the green spectral region with a maximum photoluminescence quantum yield of up to 93%, have narrower emission spectra, and can easily disperse in water. The size distribution of the polymer-coated NCs becomes more uniform and well-dispersed. The water dispersity and stability of these polymer-coated NCs significantly improved in comparison to the conventional silica-coated NCs. Such water-stable NCs were tested as a luminescent probe for Cu2+-ion detection in water that shows a detection limit of 18.6 μM. These outcomes are very encouraging for futuristic display technologies, bioimaging, and sensing applications.
Recently, perovskite NCs have been used as fluorophores for the detection of different metal ions, owing to their excellent emission properties.25–31 There are reports of Cu2+-ion detection in the presence of highly stable lower-dimensional perovskite NCs in aqueous media.32–34 CsPbX3 NCs have been proven to be a potential fluorescent probe for Cu2+-ion detection in organic, bio, and industrial oils.29–31,35 Most of these experiments were performed in nonpolar solvents to avoid the degradation of perovskite NCs due to their poor structural stability.36,37 These non-polar solvents are immiscible in aqueous media, which restricts metal ion detection in the biological systems or natural resources. So, highly water stable and water dispersible fluorescent probes are required such that the detection efficiency of metal ions can be improved. The perovskite NCs are usually encapsulated with oleic acid (OAc) and oleylamine (OAm) ligands, which are very dynamic and unstable. So, the NCs are very prone to degradation in the presence of heat, water, or intense UV light. It's a basic need to improve the perovskite structural stability for implementing them in real-world activities. Shelling of perovskite NCs with different stable materials is an effective way to further improve the NCs’ stability and luminous intensity. These shelling materials protect the core from external harsh environments and maintain high emission intensity and stability for a longer time period. Bhaumik et al. synthesized methylammonium lead bromide (MAPbBr3) core and layered octylammonium lead bromide [(OA)2PbBr4] shell NCs by a ligand-assisted reprecipitation (LARP) synthetic method, demonstrating better structural stability and luminescence intensity that persisted for several months.38
In succession, various research groups reported the coating of perovskite NCs with various stable shelling materials, such as lower-dimensional perovskites, metal oxide layers, metal sulfide layers, or bulky polymers.39–49 CsPbX3@Cs4PbX6 and CsPbBr3@Rb4PbBr6 core@shell NCs were also synthesized via a hot-injection method that shows higher luminescence intensity and superior photostability.50–52 The polymers are usually flexible and increase the hydrophobicity of NCs, which improves the water stability. Polyvinyl-pyrrolidone (PVP) polymer encapsulated CsPbBr3 NCs embedded in a polystyrene (PS) matrix exhibited better water resistance and were demonstrated as luminescent probes in live cells.53 PVP-coated CsPbBr3 NCs surrounded by a polymethyl methacrylate (PMMA) matrix were also explored for live-cell imaging.54N-isopropyl acrylamide (NIPAM) was also extensively exploited as a thermosensitive polymer for biomedical applications and drug delivery.55–57 Silica-coated perovskite NCs are mostly explored due to their better stability in water.48,58 This synthesis procedure required a longer reaction time for the completion of the hydrolysis and condensation processes of silane groups for the growth of a thick silica shell around the NCs. The silica-coated NCs also tend to agglomerate among themselves and become bigger particles for reduction of surface energy, resulting in non-uniform particle size distributions.42,59 These agglomerations among NCs also lead to an increase in NCs reabsorption and scattering, causing a decrease in the NCs luminous intensity and device efficiency.
Here in this work, we tried to find an easy and robust synthesis protocol that can be suitable for industrial processing. We report the synthesis of CsPbBr3 NCs via a one-pot LARP synthetic approach under normal atmospheric conditions (relative humidity level above 80%). Here, we encapsulated the CsPbBr3 NCs with different stable materials, such as SiO2, PVP, or mixed PVP-NIPAM polymers, and then investigated their structural and emission properties. In the case of silica-coated NCs, we selected (3-aminopropyl)trimethoxysilane (APTMS) as a silica source because APTMS binds the CsPbBr3 NCs surface with their amino groups while the alkoxysilane groups hydrolyze to form silanol groups in the presence of a trace amount of water in toluene solvent during the synthesis process.48,60 Furthermore, silanol groups condensate to form silica coatings around the NCs. In the case of the polymer coating, PVP and NIPAM polymers were used as shelling materials that attach to the NC surface and help to control the NCs growth. PVP gets adsorbed to the surface of the NCs, and further, NIPAM and PVP intertwine among themselves to form a protective shell that protects the NCs core from the harsh atmosphere. OAc and OAm ligands are also added during the NCs synthesis process such that OAc ligands prevent agglomeration among the perovskite NCs, while the amino groups of the OAm ligands attach to the NCs surface and improve NCs solution stability.61 Finally, we used the most stable polymer-coated NCs as a luminescence agent to investigate their Cu2+-ion detection ability in water. Since the degradation of perovskite NCs becomes slower in water for effective polymer coating, this permits the detection of Cu2+-ions directly in water with high sensitivity. This work paves a way to detect Cu2+-ions in biological systems or natural resources.
:
OABr = 8
:
2) were injected into the PbBr2 precursor solution and mixed properly. Finally, 10 μL of APTMS was injected into the PbBr2 precursor to form the final precursor. 250 μL of the final precursor was quickly injected dropwise in a round bottom flask containing 5 mL of toluene under vigorous stirring conditions. The stirring was continued for 4 hours to complete the hydrolysis process of APTMS. The NC solution was then centrifuged at 3000 rpm for 15 min. The supernatant was discarded and the precipitate was dispersed in 1 mL of ethanol for further characterization. The NCs are renamed CPB-SiO2 for better understanding.
:
OABr = 8
:
2) were injected into the PbBr2 precursor solution and mixed properly. Finally, 50 μL of OAc and 25 μL of OAm were added to the mixture solution to form the final precursor. 250 μL of the final precursor was injected dropwise into a round bottom flask containing 5 mL toluene and 4 mg PVP under vigorous stirring. The reaction was continued for 30 min and then the reaction was stopped. The resulting CsPbBr3 NC solution (renamed PbN-1) was transferred to a centrifuge tube and then 2 mL ACN was added. The mixture was centrifuged at 6000 rpm of speed for 15 min and the precipitate was dispersed in 1 mL toluene or water for further characterization. The mixed PVP-NIPAM coated CsPbBr3 NCs were synthesized following the same method with slight modification in which the amount of PVP (∼4 mg) was kept fixed while variable amounts of NIPAM (5 mg: PbN-2, 10 mg: PbN-3, 15 mg: PbN-4, and 20 mg: PbN-5) were added.
The X-ray diffraction (XRD) pattern of CPB@SiO2 and different PbN NCs in thin-film form are demonstrated in Fig. 1. The diffraction pattern for the CPB@SiO2 NCs thin-film reveals mixed perovskite phases, i.e., 3D CsPbBr3 (monoclinic phase) and 0D Cs4PbBr6 (rhombohedral phase) crystal structures. Similar mixed-phase perovskite NCs were already reported when the silica-coated CsPbBr3 NCs were synthesized via the LARP synthesis method.10,62 Significant XRD diffraction peaks are observed at 2θ values of 15.45°, 21.76°, 30.56°, 34.7°, 37.94°, and 44.38° that correspond to the (100), (110), (002), (201), (211), and (202) lattice planes of the 3D monoclinic CsPbBr3 crystal structure (PDF #00-18-0364).10,62 The additional XRD diffraction peaks located at 2θ values of 12.91°, 20.34°, 22.66°, 25.68°, 27.77°, 28.84°, 30.55°, 34.18°, 39.26°, and 46.07° signify the (110), (113), (300), (024), (131), (214), (223), (134), (324), and (600) lattice planes of the rhombohedral Cs4PbBr6 crystal structure (PDF #01-73-2478).50,63 The contribution of rhombohedral Cs4PbBr6 phases is quite high as compared to monoclinic CsPbBr3 phases. The XRD diffraction pattern of PbN-1 NCs reveals three perovskite phases, i.e., 3D CsPbBr3 (monoclinic phase), 0D Cs4PbBr6 (rhombohedral phase), and 2D CsPb2Br5 (tetragonal phase) crystal structures. The XRD diffraction peaks obtained at 2θ values of 15.18°, 26.75°, 30.96°, and 34.17° signify the (001), (111), (200), and (210) lattice planes of the monoclinic CsPbBr3 crystal structure. Two additional XRD peaks observed at 18.01° and 30.97° correspond to the (202) and (006) lattice planes of the rhombohedral Cs4PbBr6 crystal structure. Some additional XRD peaks obtained at 2θ values of 24.36°, 29.25°, 41.08°, and 46.96° correspond to (202), (213), (314), and (207) lattice planes of the tetragonal CsPb2Br5 crystal structure (PDF#25-0211).45,64 With an increase in NIPAM amount (i.e., PbN-2, PbN-3, PbN-4, and PbN-5 NCs) in the PbN-1 NCs, there is a minimal change in the monoclinic CsPbBr3 crystal phases. In contrast, an abrupt reduction in rhombohedral Cs4PbBr6 and tetragonal CsPb2Br5 crystal phases is noticed. The XRD diffraction peaks related to (OA)2PbBr4 perovskite phases can’t be detected due to the formation of a very thin shell layer and below the XRD instrument detection limit.38,48
The shape and size of the NCs are investigated using transmission electron microscopy (TEM) and high-resolution transmission electron microscopy (HRTEM) imaging. The TEM and HRTEM images of CPB@SiO2 and PbN NCs are shown in Fig. 2, and the corresponding particle size distributions are represented shown in Fig. S2 (in ESI†). The slightly blurry surfaces around the CPB@SiO2 NCs (see Fig. 2a) appeared from the adsorption of the silica coating that is compact and has a shell thickness of a few nm. The silica shells diffuse among other silica-coated NCs and transform into bigger irregular shapes. The average particle size distribution of the CPB@SiO2 NCs is 32 ± 7 nm, which is quite big in size. These NCs exhibit inter-planar spacing of 0.42 nm that corresponds to the (110) lattice planes of monoclinic CsPbBr3 crystal phases.65 In comparison, the polymer-coated PbN NCs (see Fig. 2b–f) reveal a monodisperse and uniform particle size distribution without any noticeable inter-particle agglomeration. These PbN NCs are cubic in shape and highly crystalline in nature. A similar (110) lattice plane appeared for the PbN NCs from the monoclinic CsPbBr3 crystal structures. The mean particle sizes of PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs are around 13.47 ± 3, 13.2 ± 3, 13.1 ± 3, 10.7 ± 2, and 10.2 ± 2 nm, respectively (see Fig. S2 in the ESI†). It can be seen that the particle size becomes smaller and the particle size distribution is more uniform with an increase in the amount of NIPAM polymer. It is beneficial for strong quantum confinement of charge carriers inside the NCs and hence enhances the optical properties.
![]() | ||
| Fig. 2 TEM and HRTEM (inset) images of (a) CPB@SiO2, (b) PbN-1, (c) PbN-2, (d) PbN-3, (e) PbN-4, and (f) PbN-5 NCs. | ||
The UV-vis absorption spectra of all the NCs in the solution phase are shown in Fig. 3a. The absorption spectrum of CPB@SiO2 reveals a band edge peak at 507 nm originated due to 3D CsPbBr3 perovskites and a minor peak at 320 nm that appeared from 0D Cs4PbBr6 perovskites.11 The PbN NCs demonstrate nearly similar absorption spectra while more intense, sharper, and well-defined absorption band edges are observed. The scattering effect of CPB@SiO2 NCs is much higher as compared to PbN NCs because of the bigger particle sizes of CPB@SiO2 NCs.66,67 The band edge absorption peaks of PbN NCs are slightly redshifted with increasing the NIPAM polymer. The PL emission spectra of CPB@SiO2 NCs (dispersed in ethanol) and PbN NCs (dispersed in toluene) are shown in Fig. 3b. The corresponding photographic images of all NCs under a UV lamp are shown in the inset of Fig. 3b. The CPB@SiO2 NCs emit a cyan-green color emission with a PL peak position at 494 nm. These NCs showed emission PLQY up to 63% with an FWHM of 31 nm. The low emission intensity of the CPB@SiO2 NCs is resulted due to the presence of unwanted Cs4PbBr6 phases that don’t contribute to the radiative recombination. The polymer-coated PbN NCs are more luminescent compared to silica-coated NCs due to the reduction of the Cs4PbBr6 phases. The PbN NCs also reveal narrower emission spectra and better emission intensity, denoting efficient radiative recombination and higher color purity. The emission peak for PbN-1 NCs is obtained at 513 nm with a very narrow FWHM of 21 nm. Initially, with the addition of NIPAM polymer up to a certain limit, the emission intensity of the PbN NCs was increased. The further increment of NIPAM polymer resulted in a reduction of the NCs PL intensity. The binding constant of the NIPAM was estimated from the change in the emission intensity of the PbN NCs with an increase in NIPAM concentration.68 The binding constant was calculated from the intercept of the plot and it comes close to 8787 M−1 (see Fig. S4, ESI†). Among all these PbN NCs, the PbN-3 NCs demonstrate the highest emission intensity with a maximum PLQY up to 93%. The CIE color coordinates of the CPB@SiO2 and PbN-3 NCs are calculated as (0.071, 0.395) and (0.079, 0.723), respectively (see Fig. S3 in the ESI†). The subsequent information regarding the PL peak position, FWHM, and PLQYs of all NCs is tabulated in Table 1.
| Name of the NCs | PL peak position (nm) | FWHM (nm) | PLQY (%) |
|---|---|---|---|
| CPB@SiO2 | 494 | 31 | 63 |
| PbN-1 | 513 | 21 | 83 |
| PbN-2 | 513 | 21 | 87 |
| PbN-3 | 513 | 22 | 93 |
| PbN-4 | 515 | 21 | 81 |
| PbN-5 | 515 | 20 | 78 |
We performed Fourier transform infrared spectroscopy (FTIR) analysis for all NCs, and the subsequent plots are represented in Fig. 3c. The spectrum for CPB@SiO2 NCs reveals strong absorption peaks located at 1107 and 754 cm−1 due to antisymmetric stretching of Si–O–Si bonds and symmetrical stretching of Si–O bonds, respectively.59,60 The additional peaks at 2927 and 2874 cm−1 appeared due to asymmetric and symmetric stretching of C–H bonds, respectively. The enrichment of the Si–O–Si and Si–O vibration peaks confirms the silica coating around the NCs after the hydrolysis process. The FTIR spectra for the PbN NCs reveal strong absorption peaks at 1294, 1650, and 3500 cm−1 corresponding to C–N, C
O, and N–H bonding vibrations of the PVP and NIPAM polymers, respectively.53–56 These vibration peaks confirm the presence of a polymer coating around the PbN NCs. There is also an absorption peak at 3100 cm−1 corresponding to –OH stretching vibrations from the presence of OAc. Additionally, the absorption peak intensities at 1650–1660 and 3500 cm−1 became intense with an increase in NIPAM polymer (PbN-4 NCs) compared to without NIPAM (PbN-1 NCs), revealing stronger C
O bonding interactions and N–H bonding vibrations, respectively. There was also a decrease in peak intensity at 3100 cm−1 with an increase in NIPAM polymer in the PbN-1 NCs, revealing the weakening of the –OH bonds.
The PbN NCs can easily be dispersed in water and maintained their luminescence properties for several days. The photographic image of the water dispersed PbN NCs under a UV lamp is shown in Fig. S5 (in the ESI†). We examined the water stability of the CPB@SiO2 and PbN-4 NCs in thin-film form by dipping them into a glass beaker containing DI water. The photographic images of the thin-films under a UV lamp are shown in Fig. 3d. The silica-coated NCs tend to agglomerate among themselves on the glass substrate and result in non-uniform film morphology. After dipping the CPB@SiO2 NCs thin-film into DI water, the luminescence of the NCs quenched instantly. In comparison, the coverage of the PbN-4 NCs thin-film is relatively better, and a smooth surface was formed due to lower surface energy after polymer coating, which is a prerequisite for the fabrication of efficient thin-film based LEDs.69,70 The emission intensity of the PbN-4 NCs thin-film was retained for a longer time period, demonstrating ultra-high stability of the PbN NCs films in water. These results conclude that the coating of PVP and NIPAM polymers around the NCs significantly improves the NCs emission intensity and crystal structural stability.
Furthermore, we performed a water stability test of all NCs in the solution phase. At first, we prepared a 5 mg mL−1 concentrated CPB@SiO2 NCs solution dispersed in ethanol, and the same concentration PbN NCs solution dispersed in water (since toluene and water are immiscible). We started with 100 μL of each NCs solution in separate glass vials followed by the addition of 50 μL of DI water in sequence. We measured the amount of DI water required to completely degrade the perovskite structures, i.e., when the luminescence from the NCs was mostly quenched (PL intensity nearly zero). The PL spectra of the CPB@SiO2, PbN-1, and PbN-4 NCs for the water-stability test are shown in Fig. 4a–c and the remaining NCs are represented in Fig. S6 (in ESI†). The CPB@SiO2 NCs degrade much faster, in which the emission color started shifting from green to blue color with addition of just 50 μL DI water (PL quenched by 73%) and the total emission was quenched in the presence of 250 μL DI water (around 96% of PL quenching). The blue emission spectrum is originated from transformation of 3D perovskite structures to comparatively stable lower dimensional perovskite structures.71,72 The water stability of the polymer coated PbN NCs is significantly improved with increasing the NIPAM polymer and hardly any emission shift is noticed. Fig. 4d shows the change in PL intensity for all NCs with the addition of DI water. The PL retention percentages for CPB@SiO2, PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs are 4%, 23%, 31%, 50%, 57%, and 53%, respectively, with addition of 250 μL DI water in the corresponding NCs solutions. The PbN-4 NCs exhibit the best water stability. The emission intensity of the PbN-4 NCs remains 21% of the original PL intensity even after the addition of 1000 μL DI water. The photographic images of all the NCs solutions after the addition of DI water are shown in Fig. S7 (in the ESI†).
We also performed a water stability test for all NCs in powder form as a function of time. Here, 100 μL of DI water was added to the same amount of NC powders and kept under a UV lamp. Then we recorded the changes in emission spectra at regular time intervals in a PL spectrometer. The corresponding emission spectra of the CPB@SiO2, PbN-1, and PbN-4 NCs are represented in Fig. 5a–c and the emission spectra of the remaining samples are shown in Fig. S8 (in ESI†). Among them, the SiO2-coated NCs are least stable under direct water contact and degraded within 10 min. Fig. 5d represents the change in emission spectra of all NCs with different time intervals after the addition of DI water. However, the polymer-coated NCs maintained their emission intensity in water for longer periods of time. The PL intensity of the CPB@SiO2 NCs degrades almost 99% of its initial PL intensity within 10 min. While the PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs retained 81%, 83%, 90%, 94%, and 93%, respectively, of their initial PL intensity within the same time period. After 60 min, the PL intensity retention percentages of the PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs are recorded as 17%, 31%, 47%, 74%, and 71%, respectively. These observations conclude that the PbN-4 NCs show the best water stability. The photographic images of all NCs after the addition of DI water with regular time intervals under a UV lamp are shown in Fig. S9 (see ESI†).
We also performed a heat stability test of all NCs in thin-film form. The glass substrates were coated with different NCs to form separate thin-films and placed on a hot-plate (temperature ∼ 60 °C). The PL intensities of the NCs thin-films were recorded by a PL spectrometer as a function of time. The PL spectra of the CPB@SiO2, PbN-1, and PbN-4 NCs thin-films with different time intervals under heating conditions are shown in Fig. 6a–c, and the PL spectra of the remaining NCs are represented in Fig. S10 (see ESI†). We observed that the heat stability of the CPB@SiO2 NCs is the highest among all NCs. The retention in PL intensity is 95% after 32 min and 91% after 60 min of time. The high thermal stability of the SiO2-coated NCs is due to the lower thermal conductivity of silica.73,74 The silica shell acts as a thermal insulation layer that protects the core material against degradation in the presence of heat. Fig. 6d shows the curve representing the change in PL intensity with time. Among the polymer-coated NCs, the PbN-4 NCs also had the highest heat stability. After 32 min of time, the PL retentions for the PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs are 26%, 30%, 41%, 57%, and 37%, respectively. Similarly, after 60 min the PL retentions for the PbN-1, PbN-2, PbN-3, PbN-4, and PbN-5 NCs are 13%, 15%, 30%, 42%, and 27%, respectively. These results indicate that the heat stability of the NCs increases with a certain increase in the amount of NIPAM polymer.
The instability of the perovskite NCs in water limits the detection of metal ions in an aqueous atmosphere.36,37 The comparatively higher water stability of the PbN-4 NCs encouraged us to further investigate their capability to detect metal ions in water media. To perform the ion detection experiment, we prepared different aqueous solutions containing Ni2+, Al3+, In3+, Co2+, Fe2+, Fe3+, and Cu2+-ions. Then these solutions were added separately in the same concentrated PbN-4 NCs solution (∼5 mg mL−1) dispersed in DI water. The subsequent photographic images of the NCs solutions before and after the addition of different metal ion solutions are shown in Fig. 7a. The emission of the PbN-4 NCs solution is totally quenched with the addition of Cu2+-ion solution while the PL intensity of other NCs solutions remained almost unchanged (see Fig. 7b). The PL quenching of the NC solution in the presence of Cu2+-ions determines the detection capability of Cu2+-ions in the aqueous solution. Furthermore, we recorded the emission spectra of the PbN-4 NCs solution in the presence of different concentrations of Cu2+-ions varied from 0 to 412 μM. With the increase of the concentration of Cu2+-ions, the PL intensity of the PbN-4 NCs is monotonically decreased (see Fig. 7c and d) while the shape of the PL spectra remained unchanged or not shifted. The linear decrease in PL intensity with an increase in Cu2+-ions confirms the high detection capabilities towards Cu2+-ions in the presence of PbN-4 NCs, and the probing window is quite wide. The possible reason for quenching of PL could be due to the transfer of electrons from NCs to Cu-ions,31 or adsorption of Cu2+-ions to the NC surface.31 Several fluorescence quenching mechanisms have been explained to describe the energy or charge transfer between donor and acceptor materials, such as fluorescence resonance energy transfer (FRET), cation exchange, and electron transfer processes.75–77 There is no spectral shift observed in the case of PbN-4 NCs after the addition of Cu2+-ions (see Fig. 7c). In the cation exchange process, the emission peak usually shifts either to higher/lower energies.77 So, the possibility of the cation exchange with Cu2+-ions in PbN-4 NCs is not feasible. The absorption spectra of the acceptors and emission spectra of the donors should overlap for the FRET mechanism.78 However, no such overlap is noticed between the emission spectrum of the PbN-4 NCs and absorption spectrum of copper acetate (see Fig. S11, ESI†). Generally, the electron transfer process exhibits linear emission quenching with the increase of metal-ion concentration.31 Similar emission quenching behaviour is observed in our system. This is attributed to the special d9 electronic configuration of Cu2+-ions, which is favourable to accept an electron and shift to a comparatively stable d10 electronic configuration.79,80 A schematic diagram of the charge transfer process in the presence of Cu2+-ions is shown in Fig. S12 (see ESI†). If the Cu2+-ions come into close proximity to PbN-4 NCs, they are adsorbed on the NC surface, triggering the charge transfer from the NCs to the Cu2+-ions. Consequently, the radiative transition from the conduction band to the valence band of the NCs is inhibited and results in PL quenching of the NCs. In order to find the detection limit of Cu2+-ions, we plotted the first four lowest concentrations at which the PL intensity of the NCs solution starts quenching and linear-fitted the points. To find the detection limit, we used the (3σ/slope) formula.81,82 The slope and σ (standard deviation) are calculated from the linear fit. Using the above formula, the lowest detection limit for the detection of Cu2+-ions is found to be 18.6 μM (R2 = 0.9986) based on the slope (=0.00266) and σ (=0.01658) values. These results are extremely beneficial for Cu2+-ion detection in natural water resources and biological systems.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ma00719c |
| This journal is © The Royal Society of Chemistry 2022 |