Open Access Article
Jonathan
Ruiz Esquius
a,
Hasliza
Bahruji
b,
Michael
Bowker
*ac and
Graham J.
Hutchings
*a
aSchool of Chemistry, Cardiff Catalysis Institute, Cardiff University, Main Building, Park Place, Cardiff CF10 3AT, UK. E-mail: Hutch@cardiff.ac.uk; BowkerM@cardiff.ac.uk
bCentre of Advanced Material and Energy Science, University Brunei Darussalam, Jalan Tungku Link, Gadong BE 1410, Brunei Darussalam
cCatalysis Hub, RCAH, Rutherford Appleton Laboratory, Harwell Oxford, Didcot OX11 0QX, UK
First published on 16th February 2021
The combination of a methanol synthesis catalyst and a solid acid catalyst opens the possibility to obtain olefins or paraffins directly from CO2 and H2 in one step. In this work several PdZn/TiO2–ZSM-5 hybrid catalysts were employed under CO2 hydrogenation conditions (240–360 °C, 20 bar, CO2/N2/H2 = 1
:
1
:
3) for the synthesis of CH3OH, consecutive dehydration to dimethyl ether and further oxygenate conversion to hydrocarbons. No significant changes after 36 h reaction on the methanol synthesis catalyst (PdZn/TiO2) were observed by XRD, XAS or XPS. No olefins were observed, indicating that light olefins undergo further hydrogenation under the reaction conditions, yielding the corresponding alkanes. Increasing the aluminium sites in the zeolites (Si
:
Al ratio 80
:
1, 50
:
1 and 23
:
1) led to a higher concentration of mild Brønsted acid sites, promoting hydrocarbon chain growth.
The production of CH3OH from syngas (CO/CO2/H2) over a CuO/ZnO/Al2O3 catalyst is a mature process (250–300 °C, 50–100 bar), with an annual CH3OH production of 57 Mt,10 and increasing. Hence, renewable H2 could be easily incorporated in the CH3OH production cycle, however for the process to be CO2 neutral, CH3OH must be obtained from recycled CO2 and sustainably produced H2. Thermodynamically, CH3OH formation from CO2 and H2 is favoured at high pressure and low temperature. Nevertheless, a high temperature (>200 °C) is needed to activate CO2, which in turn results in the deactivation of Cu-based catalysts due to Cu sintering9–13 and coke deposition.14 Pd-based catalysts are employed in CO2 hydrogenation to CH3OH as a stable alternative to Cu-based catalysts.15–19
Research on Pd/ZnO catalysts confirmed the β-PdZn alloy as the active phase for CH3OH synthesis.20–23 Commercially sourced ZnO usually has a low surface area which results in large PdZn particles, and hence, to improve PdZn dispersion, supports with a higher surface area (e.g., CeO2,18 carbon nanofibers,22 carbon nanotubes,24 Al2O3,25 or TiO2 (ref. 25 and 26)) are commonly used. The higher stability of PdZn alloy catalysts allows for higher reaction temperatures, however, then CH3OH productivity is limited by the thermodynamic equilibrium whilst CO formation is favoured through the reverse water gas shift (RWGS) reaction. To increase oxygenate productivity above the limited CO2 hydrogenation to CH3OH dictated by the equilibrium, CH3OH can be simultaneously dehydrated to dimethyl ether (DME) by physically mixing a methanol synthesis catalyst with a solid acid catalyst.27–30 ZSM-5 zeolites are commonly employed as solid acid catalysts to dehydrate CH3OH to DME due to their high resistance to water, high stability and the presence of Lewis and Brønsted acid sites.31 The conversion of methanol or dimethyl ether to hydrocarbons (MTH or DMTH respectively) is a mature process that also employs ZSM-5 zeolites as catalysts (300–500 °C, 1 bar).32–34 More importantly, it has been reported that using H2 or H2O in the feed for the MTH process decreased the deactivation of several zeolites (HSAPO, HSSZ, HFER, HBEA, ZSM-5) by limiting coke deposition within structural pores, without significantly affecting the hydrocarbon chain distribution or the olefin-to-paraffin selectivity.35–37 Water is produced as a by-product in CO2 hydrogenation to CH3OH, moreover H2 is present in the feed. Hence, the synthesis of hydrocarbons from CO2 over a methanol synthesis catalyst combined with an acid catalyst with reduced coke deposition is achievable. Bonura et al.29 studied different reactor bed configurations for the direct synthesis of DME from CO2 by combining a methanol synthesis catalyst and a solid acid catalyst, and found that a physical mixture (also known as a hybrid catalyst) of Cu–ZnO–ZrO2 and H-ZSM-5 gave the highest oxygenate (CH3OH + DME) productivity. Higher oxygenate productivity was also observed for a Pd/ZnO–ZSM-5 hybrid catalyst compared to a PdZn on ZSM-5 catalyst.38 Ihm et al.39 reported the direct synthesis of hydrocarbons from CO2 + H2 on CuO/ZnO/ZrO2–ZSM-5 (Si/Al = 22) hybrid catalysts. At 400 °C and 30 bar the selectivity towards CO, oxygenates and hydrocarbons observed was 93.4, 1.8 and 4.8% respectively. C5+ products were detected, although C1 and C2 products accounted for 95.4% of the hydrocarbon product distribution. Over a ZnZrO2/SAPO catalyst at 380 °C and 20 bar (∼18% CO2 conversion), the CO selectivity was reduced to 47%, whilst C2–C4 olefins accounted for 80% of the total hydrocarbon distribution, and the remaining hydrocarbons were assigned to C2–C4 alkanes (14%), C1 (3%) and C5+ (3%).40 Light olefins synthesised on hybrid catalysts from CO2 can also undergo further reduction to their corresponding alkanes on the methanol synthesis catalyst, which effectively acts as a hydrogenation catalyst. Park et al.41 reported ethane (76.4%) as the main hydrocarbon product over a CuZnOZrO2–ZSM-5 catalyst (28 bar, 400 °C), with little formation of C3 (4.5%), C4 (0.8%) and C5+ (0.2%) products. However, as reported by Giordano, Frusteri and co-workers42,43 for CO2 conversion to DME over CuZnZr/ferrierite hybrid catalysts, Cu remains prone to severe sintering under the reaction conditions (260 °C, 30 bar). This makes catalyst stability the bottle neck of this process.
To the best of our knowledge, reports on PdZn hybrid catalysts for CO2 hydrogenation focus on DME,27,38 but no detailed attention has been paid to the produced hydrocarbons. We therefore assessed the activity and stability of diverse PdZn/TiO2–ZSM-5 hybrid catalysts under CO2 hydrogenation conditions (20 bar, <360 °C) and identified produced hydrocarbons derived from MTH and DMTH.
:
5 palladium to zinc molar ratio, Pd(acac)2 (0.43 g, 1.40 mmol), Zn(acac)2 (2.06 g, 6.93 mmol) and TiO2 (2.39 g) were physically mixed in a glass vial until homogeneous. The mixture was then transferred into a Schlenk flask, evacuated (10−3 bar) and heated (145 °C, 1 h). The as prepared materials were recovered and annealed in static air (10 °C min−1, 500 °C, 16 h). PdZn/TiO2 characterisation was performed on a portion of catalyst reduced in flowing 5% H2/Ar (400 °C, 5 °C min−1, 1 h).
:
1 will be referred to as ZSM-5(23).
:
1
:
3, 30 ml min−1), and the reactor was pressurised to 20 bar and heated to the desired reaction temperature (240, 270, 300, 320, 340 and 360 °C, 5 °C min−1, 6 h dwell). To avoid product condensation, post reactor lines and valves were heated to 130 °C. Products were analysed via online gas chromatography (Agilent 7890, fitted with FID and TCD detectors). Details of how CO2 conversion, product selectivity and productivities were calculated can be found in the ESI (eqn (S1–S11†)).
:
5 was previously reported.25–27
Firstly, the catalytic activity of PdZn/TiO2 (0.25 g catalyst diluted with 0.25 g of SiC) for CO2 hydrogenation was assessed (20 bar, CO2/N2/H2 = 1
:
1
:
3, 240–360 °C). As observed in Table S2,† raising the reaction temperature from 240 to 360 °C resulted in an increase in the CO2 conversion from 6.8 to 31.2%, accompanied by an increase in the CO selectivity (from 74.6 to 97.9%) at the expense of CH3OH selectivity (from 24.3 to 1.3%), in accordance with the reaction thermodynamics.45 Below 300 °C, CH3OH synthesis proceeded in the kinetic regime (Fig. 1a), as shown by the increase in the CH3OH productivity with temperature up to 518 mmol kgcat−1 h−1. At 300 °C, the CH3OH yield reached equilibrium (1.45% CH3OH yield),45 and hence, above 300 °C CH3OH synthesis is controlled by the thermodynamic equilibrium (Fig. 1b), as shown by the sharp decrease in CH3OH productivity. Low selectivity toward CH4 (<0.8%) and DME (<1.0%), produced by CH3OH decomposition on TiO2 (ref. 46 and 47) and CH3OH dehydration,27 respectively, was observed. Nevertheless, in the absence of ZSM-5 solid acid catalysts, no other hydrocarbons were detected.
![]() | ||
Fig. 1 (a) CH3OH, DME and CH4 productivities and CO2 conversion for CO2 hydrogenation (20 bar, 30 ml min−1, CO2/H2/N2 = 1 : 3 : 1, 240–360 °C, 6 h dwell) over PdZn/TiO2. (b) Theoretical CH3OH yield obtained from Shen et al.45 compared to experimental CH3OH yield with temperature over PdZn/TiO2. | ||
Comparable CO2 conversion and CO productivity to PdZn/TiO2 were observed for all PdZn/TiO2–ZSM-5 hybrid catalysts (Fig. 2), indicating that the activity of the methanol synthesis catalyst is not altered by the proximity of solid acid zeolites, and that ZSM-5 zeolites are not active towards the RWGS. To ensure that ZSM-5 zeolites do not act as RWGS or as CH3OH synthesis catalysts, blank ZSM-5(23) was employed for the CO2 hydrogenation reaction (Table S3†), and negligible CO2 conversion was observed at 270 °C. The efficient dehydration of CH3OH to DME occurred over all PdZn/TiO2–ZSM-5 hybrid catalysts. The highest oxygenate productivity (CH3OH + DME) was obtained at 270 °C. At this temperature almost no methanol to olefins (MTH) or dimethyl ether to olefins (DMTH) conversion takes place, with only small traces of ethane detected over hybrid catalysts with ZSM-5(50 and 80), and small amounts of higher hydrocarbons observed for PdZn/TiO2–ZSM-5(23). DME is the major oxygenate product with a selectivity close to 20%. Moreover, the total methanol productivity (CH3OH(tot)), considering that all hydrocarbons originate from CH3OH by either dehydration to DME or through the MTH/DMTH process, was higher for all hybrid catalysts compared to PdZn/TiO2 (Fig. 3).
![]() | ||
Fig. 2 CO2 conversion and CO productivity over PdZn/TiO2 and PdZn/TiO2–ZSM-5 hybrid catalysts during CO2 hydrogenation (20 bar, 30 ml min−1, CO2/H2/N2 = 1 : 3 : 1, 240–360 °C, 6 h dwell). | ||
![]() | ||
Fig. 3 CO, oxygenate and hydrocarbon selectivity and total CH3OH productivity for CO2 hydrogenation (20 bar, 270 °C, CO2/H2/N2 = 1 : 3 : 1) over PdZn/TiO2 and PdZn/TiO2–ZSM-5 hybrid catalysts. | ||
The hydrocarbon productivities and CH3OH(tot) over PdZn/TiO2–ZSM-5 hybrid catalysts can be found in Table S4.† At 300 °C, the hybrid catalysts showed higher CH3OH(tot) compared to PdZn/TiO2, thus overcoming the theoretical CH3OH yield dictated by the equilibrium. Increasing the alumina ratio in the zeolite promoted the formation of longer hydrocarbons. The presence of aluminium sites is related to Brønsted acid sites with mild acidity, and hence, a higher concentration of Brønsted acid sites promotes chain growth via the hydrocarbon pool mechanism.33,48 Light olefins produced as intermediates in MTH49 undergo further hydrogenation over PdZn/TiO2, yielding the corresponding alkanes (ethane and propane); a mixture of n-butane and 2-butene was observed, whilst only olefins were detected in the C5 fraction (1-pentene and 2-cis/trans-pentene). Thus, when PdZn alloys are used for the synthesis of hydrocarbons from CO2via a methanol mediated route over hybrid catalysts, they behave as methanol synthesis catalysts but also as olefin hydrogenation catalysts, limiting hydrocarbon chain growth as also reported for Cu-based catalysts.49–51 CH3OH(tot) over hybrid catalysts is higher compared to PdZn/TiO2 at any temperature, with total CH3OH productivity surpassing the equilibrium yield above 300 °C. The highest total CH3OH productivity for hybrid catalysts was observed in the 270–300 °C range; hybrid catalysts with ZSM-5(80 and 50) gave the highest oxygenate productivity (CH3OH and DME), while ZSM-5(23) led to higher hydrocarbon productivity (Fig. 4) via faster MTH/DMTH. Although the total CH3OH productivity was higher than the equilibrium yield, above 300 °C, the hydrocarbon productivity is limited by CH3OH availability which leads to a decrease in the total CH3OH productivity at higher temperatures. The hydrocarbon selectivity based on MTH/DMTH showed that increasing the aluminium concentration in ZSM-5 in the hybrid catalyst resulted in improved selectivity towards higher hydrocarbons (Table S5†). In the 320–340 °C temperature range ethane and propane accounted for 50% of MTH/DMTH product selectivity for all hybrid catalysts. Note that the real CH4 selectivity via the MTH and DMTH process is lower than the reported values, since CH4 is also produced as a by-product in CH3OH decomposition on PdZn/TiO2.47
The stability of the PdZn phase in the PdZn/TiO2 methanol synthesis catalyst was assessed through XAS, XRD and XPS characterisation pre- and post-reaction (20 bar, CO2/H2/N2 = 1
:
3
:
1, 30 ml min−1, 240–360 °C, 6 h dwell, 36 h reaction). Extended X-ray absorption fine-structure spectroscopy (EXAFS) at the Pd K-edge was employed to detect structural and electronic changes in the PdZn phase after reaction. No noticeable differences were observed between the EXAFS spectra up to 3.5 Å of PdZn/TiO2 after pre-reduction (5% H2, 400 °C, 1 h) and after CO2 hydrogenation at up to 360 °C (Fig. 5a). Bulk Pd has a cubic structure with a Pd–Pd bond distance of 1.75 Å, whilst the β-PdZn alloy has a tetragonal structure. As expected for the intercalation of a Zn atom between two Pd atoms, on average shorter bond distances for the first coordination shell compared to bulk Pd were observed (shorter Pd–Zn bond distance compared to the Pd–Pd distance in Pd foil).59 Moreover, comparison with a PdO standard could suggest the presence of a Pd–O bond at 2.02 Å, with the concomitant but lower intensity Pd–O–Pd bond at 3.41 Å in the second coordination shell.60 This could be attributed to oxidation of the first atomic layer of the PdZn alloy in contact with air.53 Peak fitting using Artemis44 allowed us to obtain the Pd–Pd and Pd–Zn bond distances and the Pd coordination environment (Table 1). Details of the fitting can be obtained from Table S6.† Based on previous reports, PdZn alloy formation begins at the surface of Pd nanoparticles via hydrogen spillover to adjacent ZnO, and the alloy grows inwards, generating a PdZn layer over a Pd core.53,57 Therefore, the incorporation of bulk Pd–Pd bond distances was necessary to obtain a good fit. No differences in the Pd–Zn or Pd–Pd bond distances or coordination number were observed, suggesting high bulk structural stability of the PdZn alloy under reaction conditions, as also reported by Olsbye and co-workers.38 Despite the apparent bond distance at 2.02 Å, no good fit was obtained after the introduction of the Pd–O scattering path, indicating that this contribution can be attributed to noise or to marginal PdO content.
| PdZn/TiO2 | Bond | Distance | CN | σ 2 | R f |
|---|---|---|---|---|---|
| Reduced | Pd–Zn(alloy) | 2.59 | 2.62–0.21 | 0.0047–0.0014 | 0.019 |
| Pd–Pd1(alloy) | 3.06 | 7.58 | 0.0217–0.0055 | ||
| Pd–Pd2(alloy) | 3.35 | 3.79 | 0.0215–0.0111 | ||
| Pd–Pd(metal) | 2.75 | 12 (fixed) | 0.0238–0.0030 | ||
| A.R. | Pd–Zn(alloy) | 2.60 | 2.71 | 0.0050–0.0015 | 0.020 |
| Pd–Pd1(alloy) | 3.03 | 7.52 | 0.0216–0.0068 | ||
| Pd–Pd2(alloy) | 3.31 | 3.76–0.2 | 0.0218–0.0115 | ||
| Pd–Pd(metal) | 2.74 | 12 (fixed) | 0.0220–0.0030 | ||
| Pd foil | Pd–Pd1 | 2.75 | 12 (fixed) | 0.0055–0.0002 | 0.016 |
| Pd–Pd2 | 3.89 | 6 (fixed) | 0.0097–0.0022 |
Phase changes in the β-PdZn alloy during reaction were investigated by recording the XRD pattern of PdZn/TiO2 after reduction (400 °C, 1 h) and after reaction (240–360 °C, 20 bar, 36 h). In agreement with the EXAFS analysis, no changes were observed in the (111) and (200) β-PdZn reflections at 41.2° and 44.1° respectively,15,19,27 showing the high thermal stability of bulk PdZn under the reaction conditions (Fig. 5b). Moreover, no significant changes were observed in the XRD peak at 40.1° assigned to metallic Pd (PDF 00-046-1043), which presumably is protected underneath a PdZn layer.53,57 Unincorporated Zn in the PdZn alloy is observed as ZnO at 31.7°, 34.4° and 36.3° (PDF 00-036-1451). In line with PdZn and Pd, no changes in the ZnO reflections were observed after reaction. Nevertheless, the TiO2-related reflections become more intense after reaction, suggesting an increase in the particle size of the support (Fig. S2†).
EXAFS and XRD are averaging techniques sensitive to bulk changes. Catalysis, however, is a surface process, and hence small changes at the surface greatly affect the catalytic activity. To follow surface changes in the PdZn alloy composition, the Pd(3d) and Zn(LM2) orbitals of the PdZn/TiO2 catalyst before and after reaction were analysed by X-ray photoelectron spectroscopy (XPS). The Zn(2p) orbital is not sensitive towards chemical changes (e.g. the binding energies for Zn0 and Zn2+ are reported at 1021.7 and 1022 eV, respectively),61 and as observed by XRD, the unalloyed zinc remained as ZnO, hence the Pd(3d) and Zn(LM2) orbitals were calibrated against the Zn(2p) orbital at 1022 eV. The Pd(3d) peak for PdZn/TiO2 after reduction and after reaction was centred at 335.6 eV (Fig. 6), between the binding energy values reported for metallic Pd (334.8–335.4 eV)62–64 and the PdZn alloy (335.6–336.7 eV).64–66 Peak fitting using finite Lorentzian line shapes for the Pd and PdZn peaks (including satellites) and Gaussian line shapes for the PdO peaks and satellites with a Shirley background as described previously47 indicated the presence of Pd, PdZn and PdO at 335.0, 335.9 and 337.2 eV, respectively (Fig. S3a†).54,64 The presence of Pd and PdZn was confirmed by the XRD and EXAFS bulk characterisation techniques, however bulk PdO was not observed. The broadening of the Pd(3d) peak after reaction indicated an increase in the proportion of surface PdO, suggesting that surface PdZn phase separation into ZnO and Pd occurred, with concomitant palladium passivation when in contact with air.53 No significant changes were observed in the Zn(LM2) Auger electron spectra before and after reaction (Fig. S3b†); the main peak at 998 eV with a minor satellite contribution at 991 eV was attributed to the presence of ZnO.67
![]() | ||
Fig. 6 Pd(3d) XPS analysis for PdZn/TiO2 after reduction (5% H2, 400 °C, 1 h) and after reaction (20 bar, 240–360 °C, 36 h, CO2 : H2 : N2 = 1 : 3 : 1). | ||
No significant changes in the PdZn phase were detected by EXAFS or XRD, confirming the bulk thermal stability of PdZn under reaction conditions (20 bar, 240–340 °C, CO2/H2/N2 = 1
:
3
:
1, 36 h). However some surface PdZn phase separation into Pd and ZnO was suggested by the XPS characterisation. Coke deposition is often reported as the main deactivation mechanism for MTH over acid zeolite catalysts. Coke inhibits CH3OH diffusion to the acid active sites by either filling zeolite cavities or blocking pores.34 Zeolites can be regenerated at high temperature (500–600 °C) by oxidising deposited coke to CO2 with oxygen.68 To assess the extent of coke deposition during CO2 hydrogenation (20 bar, 240–340 °C, CO2/H2/N2 = 1
:
3
:
1, 36 h) over PdZn/TiO2–ZSM-5 hybrid catalysts, TGA-MS was performed on fresh and spent catalysts (Fig. S4†). The mass loss observed below 200 °C can be assigned to physi/chemisorbed water. Just above 200 °C, an extra 1 wt% mass loss compared to the fresh samples was observed for the PdZn/TiO2–ZSM-5(80 and 50) hybrid catalysts with a corresponding release of CO2, which could be assigned to coke deposits with high oxygen content as reported for CH3OH conversion to olefins over ZSM-5.69 No additional mass loss at higher temperature, which would be assigned to coke deposits with low oxygen and hydrogen content (e.g. aromatics), was detected.69 No coke deposition was detected for PdZn/TiO2–ZSM-5(23). This should not be interpreted as ZSM-5(23) being less sensitive to coke deposition, since a higher concentration of acid sites generally leads to faster deactivation,70 but instead the initial rate of coke formation might be slower in this system. This might be attributed to the presence of H2O and H2 in the feed35–37 as well as the low concentration of CH3OH throughout the catalyst bed.69
:
3
:
1, 30 ml min−1, 36 h) was confirmed by XAS and XRD. However XPS suggests that some surface PdZn separation into Pd and ZnO occurred during the reaction.
Footnote |
† Electronic supplementary information (ESI) available: XRD, pore size and surface area for commercial ZSM-5 after activation (550 °C, 6 h). CO2 reaction metrics. CO2 hydrogenation activity over PdZn/TiO2 at different temperatures, CO2 hydrogenation over ZSM-5 (23 : 1). Productivities and hydrocarbon selectivity based on MTH/DMTH over PdZn/TiO2–ZSM-5 hybrid catalysts. EXAFS fitting parameters. XRD and XPS post reaction PdZn/TiO2 characterisation. Coke determination by TG-MS. See DOI: 10.1039/d0fd00135j |
| This journal is © The Royal Society of Chemistry 2021 |