Open Access Article
Chao Zhu,
Yehai Yan
,
Fan Wang,
Jian Cui,
Shuai Zhao
,
Ailin Gao and
Guangfa Zhang
*
Key Laboratory of Rubber-Plastics, Ministry of Education/Shandong Provincial Key Laboratory of Rubber-Plastics, School of Polymer Science and Engineering, Qingdao University of Science and Technology, Qingdao 266042, P. R. China. E-mail: gfzhang@qust.edu.cn
First published on 5th March 2019
Due to their ultrathin 2D laminated structure as well as excellent mechanical and thermal stabilities, ultrafine graphene-based nanoparticles exhibit fascinating advantages as highly-efficient lubricant additives. However, it remains a daunting challenge to achieve good and durable dispersion of these graphene-based nanoparticles in lubricating oils. Herein, we report a facile and efficient integration strategy involving particle size miniaturization, surface grafting with octadecyl alcohol (OA), and partial chemical reduction to prepare a novel long-chain alkyl functionalized ultrafine reduced graphene oxide (RGO-g-OA) with highly-dispersive capacity and superior tribological performance. The chemical composition and structural characteristics, microstructural morphology, and particle size distribution of RGO-g-OA were systematically investigated. Combining significantly improved lipophilicity derived from the long-chain alkyl grafting and partial chemical reduction with the small-size effect gave rise to outstanding long-term dispersion stability (as long as one month) of RGO-g-OA in the finished oil. Moreover, the friction coefficient and wear volume of finished oil with merely 0.005 wt% RGO-g-OA greatly reduced to 0.065 and 10
316 μm3, decreased by 9.7% and 44%, respectively, compared to those of pristine finished oil, demonstrating remarkable friction reduction and anti-wear performances. Consequently, owing to the characteristics of facile fabrication, durable dispersion stability, and superior tribological performance at an extremely low content, this novel nanoadditive shows a promising application potential in the tribology field.
Encouragingly, in recent years, employment of nanomaterials as superior solid lubricants or nanoadditives has attracted extensive attention due to their unique merits, such as smaller size and chemical and thermal stability.4,7 These nanomaterials can not only easily form a shearing thin film at the sliding contact interface and thus yield low friction, but also fill and/or repair the grooves formed on the worn surfaces, revealing comprehensive advantages for improving the tribological performances of lube oil. Graphene, as an emerging star of nano-lubricating oil additives, exhibits irresistible advantages in the area of tribology, owning to its inherently unique structural characteristics.8 Specifically, smaller size and ultrathin lamellar structure make it easily enter the mated interfaces of friction pairs, avoiding the direct contact of rubbing surfaces and thus greatly reducing friction and wear during friction processes.8 Moreover, excellent mechanical and thermal stability ensure that graphene can maintain a more stable and highly-efficient lubricating performance even under harsh tribology conditions, i.e., high pressure, high temperature, and high mechanical stresses.4 Based on these advantages, considerable efforts have been devoted to exploit graphene as a nanoadditive for enhanced friction reduction and anti-wear properties.8–10 For example, Eswaraiah et al. dispersed graphene in engine oil by probe sonication and an elevated lubricating performance was observed: the friction coefficient and wear scar diameter were reduced by 80% and 33%, respectively.11 Zhao et al. reported a polyalphaolefin lubricant oil with added graphene, which showed 30% decrease of the friction coefficient and few scratches on the rubbing surface.12 Although pristine graphene as an additive can improve the tribology properties of lubricating oil to some extent, the easy aggregation behavior of pristine graphene is a troublesome obstacle, severely restricting its widespread application.13 To overcome this limitation, the introduction of additional molecular dispersants and surface chemical modification are the two most common strategies for enhancing the dispersion capability of pristine graphene.14 However, these methods suffer from some distinct disadvantages including the following: (a) unstable molecular additives tend to decompose because of the high shear stresses and high local temperatures at the rubbing surfaces during the friction process; (b) due to the strong chemical inertness of pristine graphene, it is quite difficult to directly conduct covalent functional modification (such as surface grafting) onto its surface.15
Fortunately, graphene oxide (GO), a vital graphene derivative, has become a promising candidate as an effective lubricant additive because of its intriguing significant advantages:16,17 (I) it features 2D single atom layered structure and excellent mechanical properties; (II) its mature manufacturing technology leads to a possibility of large-scale production and low cost for practical application; (III) abundant oxygen-containing groups (such as carboxyl, hydroxyl, and epoxy groups) on GO's surface provide the crucial chemical basis for further chemical grafting modification.18 However, it should be pointed out that pure GO is not suitable for direct utilization in lubricating oils since abundant oxygenated components can greatly decrease its inherent thermal stability and also distinctly weaken its dispersion capacity in non-polar lubricant oils.19 In recent years, many methodologies have been explored to address these issues.20–24 Among them, surface grafting of long-chain non-polar groups onto GO is regarded as one of the most efficient strategies to reinforce its lipophilicity and thus increase its dispersion stability in lube oils.25–29 For instance, Shivina et al. prepared an octadecylamine grafted graphene oxide, which exhibits good dispersion capacity in hexadecane, by coupling alkylamine with the carboxylic groups in GO.30 Nurul et al. demonstrated that highly oil-dispersed GO sheets can be fabricated by introducing an organic moiety using CuAAC via click chemistry; the base oil formulated with these functionalized GO additives achieves good friction-reducing and anti-wear properties.28 Note that the particle size of graphene-based nanomaterials has great influence on their dispersion stability.31 However, dispersibility and tribological performance both affected by the synergistic effect between chemical modification and particle size of GO have been rarely reported so far.
Herein, we demonstrate an efficient integrated strategy for fabricating novel small-size and alkyl-functionalized reduced graphene oxide (RGO-g-OA) with high dispersion capacity and superior tribological performance. As illustrated in Scheme 1, the preparation procedure included three key steps: (a) mechanical crushing to yield smaller-sized GO; (b) esterification reaction using octadecyl alcohol (OA); (c) partial chemical reduction by L-ascorbic acid. The chemical composition, structural characteristics, microscopic morphology, and particle size of RGO-g-OA were comprehensively investigated. Interestingly, the resultant RGO-g-OA exhibited excellent thermal stability and long-term dispersion stability (as long as one month) in the finished oil. Moreover, the tribological performance of finished oil formulated with different weight fractions of RGO-g-OA was systematically evaluated by a reciprocating friction and wear method. A possible corresponding friction-reducing and anti-wear mechanism was discussed as well.
Typically, GO (50 mg) and DMF (2 mL) were added to a round-bottom flask (50 mL) and mixed by ultrasonication for 30 min, followed by SOCl2 (20 mL) being slowly added to the mixture. The acyl chloride reaction was then conducted at 70 °C for 24 h and the resultant product was washed with DMF by centrifugation three times to obtain acyl chlorinated graphene oxide (GO-COCl). Afterwards, triethylamine (Et3N, 2 mL) and OA (3 g) were added into the GO-COCl/DMF dispersion (2.5 mg mL−1, 20 mL) in an ice-water bath and the grafting reaction was conducted under reflux at 80 °C for 24 h. The obtained mixture was filtered to yield long-chain alkylated graphene oxide (GO-g-OA). Finally, a certain amount of L-ascorbic acid (weight ratio L-ascorbic acid/GO-g-OA = 2
:
1) was added to partially chemically reduce GO-g-OA at 80 °C for 6 h, followed by filtration washing with DMF and drying at 60 °C in an oven to acquire chemically reduced alkylated graphene oxide (RGO-g-OA). For comparison, reduced graphene oxide (RGO) treated by L-ascorbic acid without alkylate functionalization was also prepared.
C (1650 cm−1) and C
O (1720 cm−1) bonds. The O–H stretching vibrations over the region of 3700–3300 cm−1 should be attributed to the hydroxyl and carboxyl groups of GO. This result reveals that a large number of oxygen-containing functional groups, such as carboxyl, hydroxyl, and epoxy groups, were successfully incorporated into the basal plane and edge of GO. It is known that carboxyl groups are mainly distributed on the edge of GO, while other oxygenated functional groups, like hydroxyl and epoxy groups, are generally immobilized onto the plane surface of GO.32 In comparison, obvious characteristic peaks at 2927 and 2850 cm−1 are found for GO-g-OA, ascribed to the typical stretching vibrations of long-chain alkyl groups (–CH2 and –CH3). In addition, the peak strength of carboxyl groups (C
O, 1720 cm−1) in GO-g-OA exhibits a conspicuous decline compared to that of GO. Thus, we conclude that OA was successfully grafted onto the surface of GO. Moreover, for RGO-g-OA, it is observed that the peak strength of C
O shows a further discernable decrease compared with that of GO-g-OA. Simultaneously, the broad epoxide (C–O–C) peak becomes a narrow spike. These results may originate from the effective removal of the great mass of oxygen functional groups due to the chemical reduction process with L-ascorbic acid.
![]() | ||
| Fig. 1 (a) FTIR spectra of GO, GO-g-OA, RGO-g-OA; (b) 1H NMR spectrum of RGO-g-OA in deuterated DMSO (chemical shift, 2.5 ppm). | ||
Additionally, 1H NMR measurement was performed to validate the chemical structure of RGO-g-OA. As shown in Fig. 1b, four different chemical shifts, that is, at 0.85 ppm (a, –CH3), 1.23 ppm (b, –CH2), 1.76 ppm (c, –OCH2CH2–), and 4.32 ppm (d, –OCH2CH2–) can be observed, further demonstrating that the long-alkyl chain OA were successfully grafted onto GO. Furthermore, strong chemical shift at 3.35 ppm should be ascribed to other hydrogen protons located on the basal plane of RGO. Therefore, the achievements of long-chain alkane grafting and subsequent partial chemical reduction pave the way toward improved lipophilicity and dispersion stability of RGO-g-OA additive in lubricants.
The phase structures of GO, GO-g-OA, and RGO-g-OA were also examined by XRD analysis. As can be seen from Fig. 2b, for the XRD pattern of GO, an obvious (001) diffraction peak at 2θ = 11.8° is found, with an interlayer space (d-spacing) of 0.730 nm calculated by the Bragg equation.35 Compared with GO, GO-g-OA shows a new broad diffraction peak (002) at 2θ = 23.6°, corresponding to d-spacing of 0.373 nm, which is derived from the disordered restacking of mildly reduced GO sheets during the grafting process. For RGO-g-OA, the (002) diffraction peak shifts to 2θ = 24.3°, corresponding to d-spacing of 0.362 nm, which is less than that of GO-g-OA, implying that the GO-g-OA was reduced after the chemical reduction by L-ascorbic acid. Note that the (001) peak would disappear because of delamination if GO was fully transformed into RGO. Thus, in this work, the strong (001) peak remaining signifies partial/incomplete reduction of GO. Overall, it is reasonable to infer that specific hydrophobic/highly-oleophilic structure of RGO-g-OA featuring large hydrophobic graphite-like domains in the middle region and long-chain alkane groups anchored onto the edge of GO sheets was acquired after the grafting reaction and chemical reduction procedures.36,37
Additionally, it is found that particle size distribution of GO mainly ranges from 1400 to 3200 nm, while the particle sizes of RGO-g-OA vary from 250 to 650 nm; the average particle sizes of GO and RGO-g-OA are 2219 and 341 nm, respectively (Fig. 3b). Such a smaller particle size for RGO-g-OA can be attributed to effective mechanical crushing from the high-speed dispersion and strong shear forces.
![]() | ||
| Fig. 4 (a) Thermogravimetric analysis (TGA) curves of GO, GO-g-OA, and RGO-g-OA; (b) detailed weight loss values of the samples in different decomposition temperature ranges. | ||
Compared with GO, both GO-g-OA and RGO-g-OA show almost negligible weight decrease in stage I, indicating that the moisture content is very low in these two materials. The weight losses of GO-g-OA and RGO-g-OA in stage II are 14% and 13%, respectively, which is due to the decomposition of oxygen-containing functional groups. It is noteworthy that the weight loss of RGO-g-OA at this temperature range is slightly lower than that of GO-g-OA, implying that the amount of oxygen-containing functional groups on RGO-g-OA decreases after the chemical reduction process. Moreover, the weight losses of GO-g-OA and RGO-g-OA in stage III are about 16% and 17%, respectively, which can be ascribed to the decomposition of long-chain alkanes. The total weight losses of GO-g-OA and RGO-g-OA in the measurement range are 37% and 35%, respectively, which are less than that of GO (41%). These results clearly demonstrate that successful grafting of OA accompanied by subsequent chemical reduction endow RGO-g-OA with much higher thermal stability.
It is well established that durable dispersion stability of additives in lubricants is a prerequisite for their efficient lubrication performance. The dispersion stability of GO-based additives in the finished oil was examined using two testing methods (standing and intensified centrifugation) and results are presented in Fig. 5. In the current study, high-performance homemade finished oil was utilized as the lubricant base oil. As indicated in Fig. 5a, the additives GO, GO-g-OA and RGO-g-OA can be uniformly dispersed in the finished oil (mass fraction, 0.01 wt%) with the aid of sonication. Obviously, GO additives containing abundant oxygenated groups associated with ultralow lipophilicity display severe agglomeration and become fully sedimentary after standing for one month, revealing inferior dispersion stability in the finished oil. In comparison, GO-g-OA exhibited a greatly improved dispersion capacity with a slight stratification phenomenon, which suggested the high efficacy of long-chain alkane functionalization toward the dispersibility of GO-based additives. More importantly, RGO-g-OA nanomaterials retained a superior dispersion stability even after one month. Strengthened centrifugal force assessment also displays similar results (Fig. 5b), that is, both RGO and GO-g-OA additives tend to agglomerate and sediment from the lubricant substrate, whereas the RGO-g-OA possesses excellent dispersion stability with no obvious precipitation behavior. Fig. S1† further demonstrates that RGO-g-OA possesses good dispersion stability in an elevated temperature environment (such as 100 °C), implying great prospects for practical application. Such remarkable dispersion durability of RGO-g-OA is believed to originate from the synergistic effect between the significantly improved lipophilicity of graphene additives, arising from long-chain alkyl (OA) grafting and partial chemical reduction, and the small-size effect (RGO-g-OA, Dmean = 341 nm).
In addition to the remarkable friction reduction effect, excellent wear-resistance performance of RGO-g-OA nanolubricant was also observed in our current work. Fig. 7 and Table 1 present the surface morphologies, cross-sectional height profiles, and volumes of the wear tracks on the surfaces lubricated with pristine finished oil and various RGO-g-OA filled finished oils. Obviously, for the worn surface of pure finished oil, as shown in Fig. 7a, a distinct dumbbell-like wear track can be observed. Meanwhile, the cross-sectional height profiles of the wear track (Fig. 7b) display dramatic fluctuation, which may be due to the extrusion and deformation effects between the measured ball and steel disc. A wear volume of 18
354 μm3 is achieved for the steel disc lubricated with pure finished oil. In contrast, the steel disks lubricated by the finished oil filled with RGO-g-OA nanoadditives display decreased wear track areas, wear heights (depth), and wear volumes compared with those of pure finished oil. These characteristic parameters exhibit similar variation trends as the friction coefficients related to the RGO-g-OA mass fractions in the finished oil. Interestingly, the finished oil containing 0.005 wt% RGO-g-OA achieves the best anti-wear performances: (a) a quite weak and blurry wear area; (b) a slight fluctuation (and lower wear depth) on the cross-sectional height profile of the wear track; (c) the smallest wear volume value of 10
316 μm3, which was decreased by 44% compared to the pristine finished oil. When the load was increased from 100 to 150 N, the finished oil with 0.005 wt% RGO-g-OA still showed good anti-wear performance compared to finished oil (Fig. S3 and Table S2, ESI†). The incorporation of 0.005 wt% RGO-g-OA into pure base oil (Fig. S4 and Table S3, ESI†) further demonstrates its high effectiveness in wear-resistance performance. Note that when the RGO-g-OA additive content reaches 0.025 wt%, the wear volume presents a significant increase and achieves a value as high as 31
639 μm3, increased by 72% compared to the pristine finished oil. Such a poor wear-resistance property is believed to originate from the excess RGO-g-OA additives, as discussed above. Consequently, in combination with the friction-reducing property, it is indisputable that the introduction of RGO-g-OA in finished oil at an extremely low amount (0.005 wt%) greatly improves both the friction reduction and anti-wear performances, demonstrating its intriguing prospect as a high-efficiency lubricant nanoadditive.
| Samples | Wear volume (μm3) | Increment |
|---|---|---|
| Finished oil | 18 354 |
0% |
| Finished oil@RGO-g-OA 0.005% | 10 316 |
−44% |
| Finished oil@RGO-g-OA 0.010% | 11 664 |
−36% |
| Finished oil@RGO-g-OA 0.025% | 31 639 |
+72% |
A mechanism for the excellent friction-reducing and anti-wear properties of RGO-g-OA nanomaterial was tentatively proposed and is illustrated in Fig. 8. Due to the small-size and ultrathin structural characteristics of RGO-g-OA nanosheets, as depicted in Fig. 3, they easily enter the rubbing interfaces between the ball and steel disc, thereby promoting the lubricating oil to form a discontinuous, thin and unstable oil film at the initial stage of the friction process. However, after a short run-in period, RGO-g-OA nanoadditives fill the pits and grooves formed on the steel disc, facilitating formation of a continuous, thick and stable tribological film to avoid direct contact between the rubbing steel ball and disc (as evidenced by SEM and Raman spectra results in Fig. S5†). Benefiting from the filling and stable tribological shielding film, the finished oil with dispersed RGO-g-OA nanolubricants endows surfaces with superior friction-reducing and wear resistance performances.
316 μm3, by 9.7% and 44%, respectively, in comparison with those of pristine finished oil. Such outstanding lubrication properties should be attributed to the fact that the ultrafine RGO-g-OA can form an intact protective tribology film between rubbing surfaces to prevent them from direct contact, thereby reducing friction and wear during the friction process. These observations demonstrate the highly-desirable effectiveness of RGO-g-OA nanocomposite for enhanced dispersibility and suggest its utilization as an efficient lubricant additive toward high-performance tribological applications.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra00433e |
| This journal is © The Royal Society of Chemistry 2019 |