Preparation of carbon-based hybrid particles and their application in microcellular foaming and flame-retardant materials

Zhicai He a, Zhengping Zhaob, Shengwei Xiao*a, Jintao Yangc and Mingqiang Zhong*c
aCollege of Medicine and Chemical Engineering, Taizhou University, Taizhou 318000, Zhejiang, P. R. China. E-mail: xiaoshengwei@hotmail.com; Fax: +86 576 88660177; Tel: +86 576 88660177
bZhijiang College, Zhejiang University of Technology, Hangzhou 310014, P. R. China
cCollege of Materials Science and Engineering, Zhejiang University of Technology, Hangzhou 310014, P. R. China. E-mail: zhongmingqiang@hotmail.com; Fax: +86 571 88320856; Tel: +86 571 88320856

Received 10th April 2018 , Accepted 27th June 2018

First published on 25th July 2018


Abstract

Polymeric microcellular foams with high strength and light weight are very important for industrial applications. However, regulating their cell structure and their weak flame retardancy are problematic. We designed single-arm POSS-based ionic liquids ([bel-POSS][PF6]), and constructed hybrid composites based on physical interaction between ionic liquids and carbon-based materials in PS microcellular foaming. Ionization of bel-POSS could result in a quaternary ammonium reaction and ion-exchange reaction, and the carbon materials exhibit good dispersion through blending. The prepared hybrid composites showed high CO2 adsorption. Conical calorimeter tests showed that PS composite materials could reduce the heat release rate, total heat release, toxic gases (CO2 and CO) release, and amount of smoke generated. These carbon materials could affect PS micropore structure, including the cell diameter and density. Upon addition of 5 wt% of carbon materials, the hole diameter decreased by >50%, and the hole density increased nearly ten folds.


1 Introduction

Due to their high strength and light weight, polymeric microcellular foams have garnered considerable attention. Compared with non-foam polymeric materials, such microcellular foams exhibit advantageous mechanical and physical properties.1–4 However, polymeric microcellular foams have weak flame-retardant properties and release toxic gases during combustion, which can have negative effects on humans and the environment.5 The conventional solution is to add certain flame retardants, but this usually affects the cell structure and properties of the foam materials. Hence, application of flame-retardant microcellular foams combined with cell-structure regulation with flame-retarding capabilities merits investigation.

Carbon materials can endow foaming materials with specific properties, including conductive, dielectric and electromagnetic shielding. Moreover, it can further improve cell structure, cell density and flame retardancy.6–9 Hence, it is necessary to: (i) establish a connection between pore-structure regulation and flame retardancy; (ii) explore high-performance polymer microporous foams that integrate structural regulation, functionalization, and flame retardancy using carbon materials.

During the foaming of composite materials, the dispersion of carbon materials has a decisive role in heterogeneous nucleation, functionalization and flame retardancy.10,11 Usually, carbon materials tend to agglomerate due to van der Waals forces unless modified through chemical grafting12–14 and physical blending.15–17 Chemical modification can damage the structure and function of carbon materials, and such modification enhances complexity simultaneously. The efficiency of flame retardants is inhibited significantly if carbon materials are added to a single flame-retardant system. Based on these disadvantages, it is necessary to introduce other flame retardants to achieve synergistic flame retardancy. For example, grafting or loading hexachlorocyclotriphosphazene (HCCP), octa(aminophenyl) caged silsesquioxane, or Ni–Fe layered double hydroxide on the surface of graphene oxide (GO) can induce GO catalytic carbonization and capture free radicals.12,18,19 Studies have revealed that polyhedral oligomeric silsesquioxane (POSS) and ionic liquids (ILs) exhibit CO2-philic and heterogeneous nucleation,20 which can improve the cell structure. POSS and ILs show good thermal stability and flame retardancy, which can reduce heat release during combustion and promote the formation of a highly antioxidant cracking layer.

Based on the studies above, we designed and fabricated a hybrid system by coupling carbon materials with POSS to maintain the complete structure of carbon materials. This as-prepared hybrid system was used for supercritical CO2 (scCO2) microporous foaming. We hoped that this strategy would lead to local enrichment of CO2 on carbon materials, improve heterogeneous nucleation efficiency, regulate cell structure, and allow the synergistic flame retardancy of POSS and carbon nanoparticles to be realized. To achieve this concept, physical interaction was established between POSS and carbon materials to enable effective combination and structural regulation. Fortunately, the coexistence of π–π conjugation and π-cations enabled tight interactions between ILs and carbon materials.21 POSS-based ILs were designed, synthesized and characterized. The π–π and π-cation interactions between ILs and carbon nanoparticles were used to construct carbon-based hybrid materials, and their dispersion, scCO2 enrichment, nucleating efficient, and flame retardancy were investigated. The integration between cell-structure regulation and flame retardancy could provide new perspectives for fabricating multi-functional microporous foaming materials.

2 Experimental

2.1 Materials

Chlorobenzylethyllsobutyl POSS (C37H73O12Si8, FW 970.11) was purchased from Hybrid Plastics (Hattiesburg, MI, USA) and was used as received. Carbon nanotubes (CNTs), GO, sodium iodide (NaI), triethylamine (TEA), potassium hexafluorophosphate (KPF6), hydrazine monohydrate and styrene (St) were obtained from Aladdin Reagents (Shanghai, China). Acetonitrile (CH3CN) was purchased from Shanghai Ling Feng Chemical Reagents (Shanghai, China) and was used as received. Polystyrene (PS) was obtained from Zhenjiang Qi Mei Chemicals (Zhenjiang, China). CO2 was supplied by Hangzhou Jingong Gas (Hangzhou, China).

2.2 Sample preparation

2.2.1 Synthesis of POSS-based IL. Benzylethyllsobutyl POSS hexafluorophosphate ([bel-POSS][PF6]) (2.9103 g, 3 mmol) and 300 mL of CH3CN were added to a flask equipped with a magnetic stirrer. After complete dissolution of the powder, TEA (3.036 g, 30 mmol) and NaI (0.4497 g, 3 mmol) were added to the solution mentioned above. The mixed reactants were stirred for 24 h at 82 °C, and then KPF6 (3.036 g, 30 mmol) was added to the reaction at 82 °C for 24 h under magnetic stirring. After completion of the reaction, the solvent was removed by vacuum distillation. A white powder was collected after water washing and dried in a vacuum at 80 °C for 24 h (3.3547 g, 94.7%). The synthetic route is shown in Fig. 1.
image file: c8ra03007c-f1.tif
Fig. 1 Synthesis of [bel-POSS][PF6].

[bel-POSS][PF6] 1H NMR (CDCl3 400 MHz, ppm): 7.31 (4H, Ph), 4.32 (2H, N–CH2–Ph), 3.25 (6H, N–CH2–), 1.58 (7H, –CH–Me2), 1.47 (9H, CH3, N–(CH2CH3)3), 1.27 (2H, –CH2–Ph), 0.98 (42H, –CH3), 0.63(14H, Si–CH2–).

Mass spectra (MS data): (electrospray ionization, ESI+) m/z 1034.5 [bel-POSS]+, (ESI−) m/z 145.0 [PF6].

2.2.2 Preparation of CNTs hybrid materials and RGO hybrid materials. A typical process for the fabrication of RGO hybrid materials was followed. For [bel-POSS][PF6]/RGO, 0.3 g of GO and 300 mL of deionized water were added to a 500 mL flask equipped with magnetic stirring. Uniform dispersion of GO solution in deionized water was achieved by ultrasonic treatment. Then, 0.6 g of [bel-POSS][PF6] and 3 mL of hydrazine monohydrate were added to the suspension and magnetic stirring was carried out at 100 °C for 24 h. After completion of the reaction, the solvent was removed by centrifugation and the black powder was collected, water-washed and dried in vacuum at 80 °C for 24 h (0.8551 g, 95.01%).

The preparation of CNTs hybrid materials was similar to that of RGO hybrid materials except that RGO replaced CNTs and hydrazine was not added. Fig. 2 illustrates a typical synthetic route of CNTs hybrid materials and RGO hybrid materials.


image file: c8ra03007c-f2.tif
Fig. 2 Preparation of carbon-based hybrid particles.
2.2.3 Preparation PS composites. Pure PS and PS composites were made into cylindrical bars using a micro twin-screw extruder operating at 190 °C.
2.2.4 scCO2 foaming process. A batch foaming process was conducted in a high-pressure vessel. The samples was placed in a vessel filled with CO2 and saturated at 100 °C and 13.8 MPa for 12 h. Then, the pressure was released rapidly in 0.5 s and foam morphology fixed by cooling in an ice–water mixture.

2.3 Measurement and characterization

1H NMR spectra were measured on an AVANCE III (500M) NMR spectrometer (Bruker, Billerica, MA, USA) using CDCl3 as the solvent. Molecular weight was determined on a 6210 time of flight liquid chromatography/mass spectrometry (TOF LC/MS) system (Agilent Technologies, Santa Clara, CA, USA) using CH3CN as the solvent. Fourier transform infrared (FT-IR) spectra were recorded on a Nicolet 6700 IR spectrometer (Thermo Scientific, Waltham, MA, USA) with a continuum microscope. The glass transition temperature (Tg) of pure PS and PS composites was measured by differential scanning calorimetry (DSC) using a TA-Q100 system (TA Instruments, New Castle, DE, USA). For DSC measurement, 10 mg of sample in an aluminum crucible was heated from 40 °C to 280 °C at 10°C min−1 under N2 flow of 10 mL min−1. The heat release rate of pure PS and PS composites was measured by a cone calorimeter. A two-roll mill and press machine was used for sample preparation (100 × 100 × 2 mm3). A flame-retardancy test was done on a cone calorimeter (Stanton Redcroft, London, UK). The test standard was ISO 5660 with heat flux of 35 kW m−2. The morphology of pure PS and PS composites was observed by scanning electron microscopy (SEM) using an S-4700 system (Hitachi, Tokyo, Japan). Samples were fractured in liquid nitrogen, and the fracture surface was sputter-coated with Au. Images were acquired at an accelerating voltage of 10 kV and a working distance of 8 mm.

The high-pressure solubility of CO2 in pure PS and PS composites was measured by a gravimetric method. Samples were saturated by CO2 at 13.8 MPa and 35 °C. Then, they were removed rapidly from the vessel for weighing, and the mass losses of samples with time were recorded. The CO2 solubility of carbon hybrid particles at atmospheric pressure was measured by a thermogravimetric analyzer (SDT Q600; TA Instruments). Samples in aluminum crucibles were at 40 °C for 60 min under CO2 flow of 10 mL min−1, and the weight gain of samples with time was recorded.

The average cell diameter and cell density were calculated using DigitalMicrograph® (Gatan, Pleasanton, CA, USA) software. Non-circular cells were assumed to have a circular shape when calculating sizes. The cell density (N0) is the number of cells per cubic centimeter of foamed samples, and was determined using the following formula:

image file: c8ra03007c-t1.tif
where D is the average cell diameter, ρf is the density of the foam sample measured according to the American Society for Testing Materials (ASTM-D792), and ρ is the density of the unfoamed sample (ρPS = 1.04 g cm−3).

3 Results and discussion

3.1 Characterization of POSS-based IL and hybrid particles

The pure POSS-based IL ([bel-POSS][PF6]) was synthesized by combination of a quaternization reaction and ion-exchange reaction. Then, a hydrazine-monohydrate reduction method and solution blending were applied to prepare RGO hybrid materials and CNTs hybrid materials, respectively. Fig. 3 displays the FT-IR spectra of as-obtained hybrid materials. For pure sin POSS, the characteristic peaks at 744 cm−1 and 1100 cm−1 were attributed to CH2–Cl and Si–O–Si, respectively. A characteristic peak at 2975 cm−1 was attributed to the stretching vibration of surface-adsorbed CO2. For [bel-POSS][PF6], the intensity of the characteristic peak at 744 cm−1 was smaller, which was due mainly to the quaternization of CH2–Cl. This result revealed that [bel-POSS][Cl] was synthesized with the feature of an unspent CH2–Cl group. A new characteristic peak ascribed to [PF6] appeared at 839 cm−1, which was an indicator of an ion-exchange reaction between [bel-POSS][Cl] and KPF6. This result further confirmed that [bel-POSS][PF6] had been prepared. Hydrazine hydrate-reduced RGO hybrid materials and CNTs hybrid materials exhibited similar FT-IR spectra with that of [bel-POSS][PF6], which showed the hydroxyl groups on GO were reduced and carbon materials (RGO and CNTs) and [bel-POSS][PF6] had combined physically.
image file: c8ra03007c-f3.tif
Fig. 3 FT-IR spectra of bel-POSS, [bel-POSS][PF6], [bel-POSS][PF6]/RGO and [bel-POSS][PF6]/CNTs.

The influence of RGO hybrid materials and CNTs hybrid materials on the thermal properties of PS were demonstrated using DSC. The DSC curves of pure PS, [bel-POSS][PF6] and composite materials are shown in Fig. 4. The Tg (which represents the upper temperature for polymer application) was obtained from DSC curves. The Tg of pure PS was 105.1 °C, and [bel-POSS][PF6] had good heat resistance and melted directly at 232.3 °C. Upon combination of the PS composites of hybrid particles and [bel-POSS][PF6], the Tg of the corresponding composites was between the Tg of pure PS and that of [bel-POSS][PF6]. When 5 wt% of the RGO hybrid particle was used, the Tg of the composite was 105.9 °C (about 0.8 °C higher than that of pure PS) and another melting temperature appeared at 226.8 °C, which was attributed to the effect of [bel-POSS][PF6]. A similar trend for the Tg of PS/5% CNTs hybrid particle was observed when a 5 wt% CNTs hybrid particle was employed, and the Tg of the composite was 106.1 °C, and the fictive temperature (Tf) was 228.1 °C. Generalized compatibility theory suggests that partially compatible systems have two Tg values, that the two Tg peaks are closer than the Tg peak of each polymer, and that there is a certain degree of diffusion of molecules (or segments) between the two phases. Therefore, there is a certain compatibility between PS, RGO hybrid particles and CNTs hybrid particles, and the hybrid particles can be well dispersed in PS.


image file: c8ra03007c-f4.tif
Fig. 4 DSC curves of pure PS, PS/5% RGO hybrid particle, PS/5% CNTs hybrid particle and [bel-POSS][PF6].

3.2 CO2 adsorption of carbon hybrids

The atmospheric adsorption of CO2 by carbon hybrid materials was assessed by TGA. As shown in Fig. 5, when the hybrid particles were immersed in CO2, the weight of the samples increased gradually with increasing adsorption time. The two hybrid samples displayed a fast adsorption rate initially. As time increased, adsorption became slower. Comparison of the CO2 adsorption properties of graphene hybrids and CNTs hybrids revealed that the latter had a stronger adsorption effect on CO2 in comparison with graphene hybrid materials. Adsorption of CNTs hybrids was always greater than that of graphene hybrids. When the samples were soaked in CO2 for 1 h, the CO2 adsorption rate of CNTs hybrid particles reached 3.25 wt%, which was better than that of RGO hybrid materials (2.72 wt%).
image file: c8ra03007c-f5.tif
Fig. 5 CO2 adsorption of carbon nanoparticle hybrid particles (1 atm, 40.0 °C).

3.3 Dispersion of carbon hybrid particles in styrene

In general, to improve the dispersion of carbon materials in polymers, they are modified to reduce the tendency of van der Waals forces to cause agglomeration. Hence, it is highly desired to use π–π and π-cation interactions between single-arm POSS-based ILs and carbon materials. To investigate the dispersion of hybrid materials, the as-fabricated samples were dissolved in St solution (Fig. 6). After stewing for 12 h, the [bel-POSS][PF6]/CNTs and [bel-POSS][PF6]/RGO hybrid materials continued to exhibit uniform dispersion in the St solution with only slight delamination, indicating moderate compatibility between the carbon materials and St. This strategy facilitated the dispersion of carbon materials in the PS matrix, and acted as heterogeneous nucleation in the foaming process.
image file: c8ra03007c-f6.tif
Fig. 6 Dispersion of carbon hybrid particles in styrene solution (12 h).

3.4 CO2 absorption of pure PS and PS composites

The solubility of CO2 in pure PS and the PS composites at room temperature was measured using a gravimetric method. Samples were saturated by CO2 at 13.8 MPa at 350 °C for 12 h and then collected rapidly from the vessel for weighing. Mass losses of samples with time were recorded (Fig. 7). Pure PS, PS/5% RGO hybrid materials and PS/5% CNTs hybrid materials showed a linear relationship between the CO2 concentration and square root of desorption time. CO2 diffusion obeys Fick's law, so the initial solubility in pure PS and PS composites can be obtained (Fig. 7) through fitting and extrapolation of the curves. The initial solubility towards CO2 absorption using PS/5% CNTs hybrid materials was 11.41%, 10.63% for PS/5% RGO, and 10.63 wt% for pure PS, respectively. Enhancement of CO2 solubility could be attributed to the affinity of carbon materials and POSS-based IL. Moreover, the capacity for CO2 adsorption of CNTs hybrid materials was slightly better than that for RGO hybrid materials. CO2 desorption for pure PS was the slowest and only 3.75 wt% CO2 was detached in 30 min. The CO2 desorption rate was accelerated considerably when carbon materials were added into the PS matrix, with 5.78 wt% of CO2 being detached in PS/5% RGO, and 8.80 wt% in CNTs hybrid materials.
image file: c8ra03007c-f7.tif
Fig. 7 CO2 solubility in pure PS and PS composites (13.8 MPa, 35 °C).

3.5 Flame retardancy of PS composites

A carbon hybrid materials flame-retardant system was designed to improve its flame retardancy. Its heat release rate (HRR), total heat release (THR), ignition time (ITT), specific extinction area (SEA), CO2 release rate, and CO release rate were evaluated using a cone calorimeter. Fig. 8 shows the HRR and THR for pure PS and PS composites. Data from Fig. 8 show the peak heat release rate (pkHRR) for pure PS to be 1670.1 kW m−2, and THR to be 149.6 MJ m−2. After adding 5 wt% CNTs hybrid particles, the pkHRR and THR were reduced to 1068.5 kW m−2 and 94.4 MJ m−2, respectively, a reduction of 36.02% and 36.9%; addition of 5 wt% RGO hybrids reduced the values by 39.97% and 42.9%, respectively.
image file: c8ra03007c-f8.tif
Fig. 8 The heat release rate (HRR) and total heat release (THR) of pure PS and PS composites.

Table 1 shows the ITT, pkHRR, THR, average specific extinction area (Av-SEA), peak CO2 release rate (p-CO2) and peak CO release rate (p-CO) for the cone calorimeter test. Data from Table 1 reveal that, after addition of carbon hybrid materials, the ITT of the composite material decreased slightly. That is, the time required for the material surface to be heated until the material continued to burn became shorter and the material became easier to burn. However, the HRR and total amount of heat released from the composite material were reduced significantly. This result suggested that the heat of combustion of the material was reduced, and that the fire risk was also reduced. The SEA denotes the smoke produced by a volatile material of unit mass, and the value of SEA is related positively to the amount of smoke produced. The Av-SEA of pure PS was 885 m2 kg−1, and that of CNTs hybrid and RGO hybrid materials decreased to 387 m2 kg−1 and 306 m2 kg−1, respectively. These findings suggested that carbon hybrid materials exhibited effective smoke suppression.

Table 1 Values using the cone calorimeter test
Sample name ITT (s) pkHRR (kW m−2) THR (MJ m−2) Av-SEA (m2 kg−1) p-CO2 (g s−1) p-CO (g s−1)
Pure PS 60 1670.1 149.6 885 0.62 0.018
PS/5% CNTs 55 1068.5 94.4 387 0.41 0.011
PS/5% RGO 50 1002.6 85.4 306 0.37 0.010


These data suggested that carbon hybrid materials could reduce the HRR of PS significantly and had good smoke-suppression properties. POSS is an organosilicon flame retardant with catalytic-carbonization and smoke-suppression properties. ILs have a phosphorus–nitrogen synergistic effect. This effect is functionalized by releasing an inert gas to interfere with the combustion chain. This inhibits smoke generation during combustion, and the release of toxic gases (CO2 and CO) and Av-SEA are reduced significantly, thereby showing obvious vapor-phase flame retardancy. Carbon materials (CNTs and RGO) promote the formation of a uniform, dense, carbon-layer barrier when they burn, thereby preventing PS decomposition and heat transfer from the surface. Besides, the construction of carbon layer can prevent thermal-decomposition products within the material from entering the flame zone and outside simultaneously, which are the characteristic features of solid-phase flame retardants.

3.6 Foaming properties of PS composites

We examined the effect of carbon hybrid materials on cell structure, especially the effect on nucleation efficiency. Therefore, pure PS, PS/5% CNTs hybrid particles, and PS/5% RGO hybrid particles were foamed under identical conditions and the cell structure of each foamed sample compared. Fig. 9 shows the SEM images of pure PS and PS composites foamed under identical conditions; the average cell diameter, cell density, and foam density of these foams are shown in Table 2. The cell diameter of pure PS was significantly larger, and cell structures improved significantly, after addition of the carbon hybrid materials. Upon addition of 5% CNTs hybrid particles, the cell diameter decreased to 2.79 μm, and the cell density increased to 5.70 × 1010 cell per cm3. Addition of 5% RGO hybrid particles elicited similar results: the average cell diameter and cell density were 2.87 μm and 5.54 × 1010 cell per cm3, respectively. Addition of carbon hybrid particles resulted in a significant increase in the cell density of the foamed material and slightly increased foam density. The increase in cell density was due mainly to the increase in the number of cell nucleation sites, which resulted in a significant increase in the nucleation efficiency of composite materials. The increase in foam density was due mainly to the low expansion ratio of foam cells.
image file: c8ra03007c-f9.tif
Fig. 9 SEM images of pure PS and PS composite foams (100 °C, 13.8 MPa).
Table 2 Foam parameters of pure PS and PS composites (100 °C, 13.8 MPa)
Samples Average cell size (μm) Cell density (cell per cm3) Foam density (g cm−3)
Pure PS 6.16 ± 1.89 0.57 × 1010 0.31
PS/5% CNTs hybrid particle 2.79 ± 0.66 5.70 × 1010 0.37
PS/5% RGO hybrid particle 2.87 ± 0.73 5.54 × 1010 0.33


Pure PS foaming is primarily a homogeneous nucleation, the Gibbs free energy barrier (ΔG*) is related mainly to the interfacial free energy (γαβ) as well as the internal and external pressure difference (ΔP) of cells, so the nucleation efficiency is not high and the average cell diameter is large. Due to the role of carbon hybrid particles, PS composites can undergo homogeneous nucleation and heterogeneous nucleation. The latter is reflected mainly in two factors. The first factor is that the nucleation additive (CNTs hybrid particle and RGO hybrid particle) is CO2-philic; this will increase the surface contact angle (θ) between the blowing gas and solid particles and reduce the heterogeneous nucleation factor. According to nucleation theory,22 the heterogeneous nucleation factor and heterogeneous nuclear energy barrier will decrease, which is beneficial to heterogeneous nucleation efficiency. The second factor is an increase in the increase of nucleation sites. During the foaming process, [bel-POSS][PF6] and carbon nanoparticles (CNTs and RGO) are in the solid state, and can have a role in the number of heterogeneous nucleation points. Surface morphology, uniform surface modification, and uniform distribution of nucleating agents are also beneficial for heterogeneous nucleation. CNTs are typical one-dimensional carbon nanoparticles, RGOs are typical two-dimensional carbon nanoparticles, and their regular surface morphologies are favorable for nucleation and growth; moreover, CO2 absorption on their surfaces promote nucleation.

4 Conclusions

We proposed a physical composite method using single-arm POSS-based ILs [bel-POSS][PF6] and carbon materials (CNTs and RGO) to enhance PS flame retardancy and to regulate cell morphology. We demonstrated that single-arm POSS-based ILs could be prepared by quaternization and ion-exchange reaction. The hydrate reduction method using hydrazine could achieve physical recombination with carbon materials. On the basis of various characterizations, carbon hybrid materials were found to be CO2-philic and to have moderate compatibility with PS. Carbon hybrid materials had a dual role in the heterogeneous nucleation and adsorption of CO2 in this system. Addition of carbon materials into the PS matrix not only regulated the cell morphology of PS, it also achieved synergistic flame retardancy.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This study was supported financially by the Zhejiang Province Public Welfare Project (2017C31112) and the National Natural Science Foundation of China (21504079).

References

  1. J. Elsing, T. Stefanov, M. D. Gilchrist and C. Stubenrauch, Phys. Chem. Chem. Phys., 2017, 19(7), 5477–5485 RSC.
  2. Y. Lei, T. Liu, Z. Chen, A. Lu, X. Wang and X. Zhao, RSC Adv., 2014, 4(37), 19103–19110 RSC.
  3. B. Jeon, H. K. Kim, S. W. Cha, S. J. Lee, M. S. Han and K. S. Lee, Int. J. Precis. Eng. Man., 2013, 14(4), 679–690 CrossRef.
  4. J. E. Martini, F. A. Waldman and N. P. Sud, SPE ANTEC Tech Papers, 1982, pp. 674–676 Search PubMed.
  5. M. Kobes, I. Helslootb, B. De Vries and J. G. Post, Fire Saf. J., 2010, 45(1), 1–11 CrossRef.
  6. X. Mu, B. Yuan, X. Feng, S. Qiu, L. Song and Y. Hu, RSC Adv., 2016, 6, 107 Search PubMed.
  7. H. Y. Ma, P. A. Song and Z. P. Fang, Sci. China: Chem., 2011, 54(2), 302–313 CrossRef.
  8. P. G. Song, Z. H. Cao, Y. Z. Cai, L. P. Zhao, Z. P. Fang and S. Y. Fu, Polymer, 2011, 52(18), 4001–4010 CrossRef.
  9. C. Y. Bao, Y. Q. Guo, B. H. Yuan, Y. Hu and L. Song, J. Mater. Chem., 2012, 22, 23057–23063 RSC.
  10. A. Ameli, M. Nofar, C. B. Park, P. Pötschke and G. Rizvi, Carbon, 2014, 71(7), 206–217 CrossRef.
  11. S. Kim, J. S. Oh, M. G. Kim, W. Jang, M. Wang, Y. Kim, H. W. Seo, Y. C. Kim, J. H. Lee, Y. Lee and J. D. Nam, ACS Appl. Mater. Interfaces, 2014, 6(20), 17647–17653 CrossRef PubMed.
  12. C. Y. Bao, Y. Q. Guo, B. H. Yuan, Y. Hu and L. Song, J. Mater. Chem., 2012, 22, 23057–23063 RSC.
  13. M. Zhao, L. H. Meng, L. C. Ma, L. N. Ma, X. B. Yang, Y. D. Huang, J. E. Ryu, A. Shankar, T. X. Li and C. Yan, Compos. Sci. Technol., 2018, 154, 28–36 CrossRef.
  14. J. Zhang, M. Zuo, X. Lv, H. Zhang and Q. Zheng, RSC Adv., 2018, 8(26), 14579–14588 RSC.
  15. M. H. Kang, H. Y. Yeom, H. Y. Na and S. J. Lee, Polymer, 2013, 37(4), 526–532 Search PubMed.
  16. L. X. Xu, J. W. Mcgraw, F. Gao, M. Grundy, Z. Ye, Z. Gu and J. L. Shepherd, J. Phys. Chem. C, 2013, 117(20), 10730–10742 CrossRef.
  17. O. Rafeie, M. K. Razavi Aghjeh, A. Tavakoli, M. Salami Kalajahi and A. Jameie Oskooie, J. Appl. Polym. Sci., 2018, 46333 CrossRef.
  18. X. Wang, Y. Hu, L. Song, H. Y. Yang, B. Yu, B. Kandola and D. Deli, Thermochim. Acta, 2012, 543, 156–164 CrossRef.
  19. C. Bao, L. Song, C. A. Wilkie, B. H. Yuan, Y. Q. Guo, Y. Hu and X. L. Gong, J. Mater. Chem., 2012, 22(32), 16399–16406 RSC.
  20. Z. C. He, M. Q. Zhong and J. T. Yang, J. Polym. Res., 2016, 12(23), 1–5 Search PubMed.
  21. D. Duan, H. Ye, N. Meng, C. Xu, B. Han, Y. Chen, M. Zhong and L. Xu, Carbon, 2018, 136(9), 417–429 CrossRef.
  22. J. S. Colton and N. P. Suh, Polym. Eng. Sci., 1987, 27(7), 500–503 CrossRef.

Footnote