Homogeneous grafting of cellulose with polycaprolactone using quaternary ammonium salt systems and its application for ultraviolet-shielding composite films

Yongqi Yu, Xin Gao, Zeming Jiang, Wentao Zhang, Jiwei Ma, Xuejiao Liu and Liping Zhang*
Department of Material Science and Technology, MOE Key Laboratory of Wooden Material Science and Application, Beijing Forestry University, 100083, Beijing, P. R. China. E-mail: zhanglp418@163.com

Received 5th January 2018 , Accepted 5th March 2018

First published on 19th March 2018


Abstract

Microcrystalline cellulose grafted polycaprolactone (MCC-g-PCL) was successfully synthesized by ring-opening copolymerization catalyzed by 4-dimethylaminopyridine in a dual tetrabutylammonium acetate/dimethyl sulfoxide solvent system. A novel ultraviolet-shielding film based on MCC-g-PCL was prepared by introducing graphene oxide (GO). The results obtained showed that the introduction of GO not only obviously influenced the inherent structure of the MCC-g-PCL but remarkably changed the surface morphology of the composite film. Moreover, the GO/MCC-g-PCL composite showed a significant improvement in tensile strength, from 2.63 to 4.55 MPa, as well as elongation-at-break, from 6.4% to 15.5%, compared with the pure MCC-g-PCL film, owing to the strong hydrogen-bonding interaction that physically crosslinked GO with MCC-g-PCL. Importantly, GO/MCC-g-PCL composite films offered an effective high-energy light-shielding capacity; in particular MCC-g-PCL film containing 1.0 wt% GO possessed good absorbance between 200 nm and 300 nm. This study provides a framework for developing cellulose-based ultraviolet-shielding polymers and better understanding the ultraviolet-shielding mechanism.


1 Introduction

Owing to the depletion of the ozone in the Earth's atmosphere, there is a progressive increase in ultraviolet (UV) radiation on human skin.1 UV radiation from the Sun or artificial sources causes photodermatosis, acceleration of skin aging and changes to the functioning of the immune system,2–7 and is a prominent risk factor in the development of skin cancer. Thus, prevention measures must be established as UV radiation is increasingly becoming a hazard. The UV-protective properties of cellulose can be improved by UV absorbers, such as zinc oxide (ZnO) nanoparticles,7–10 which were incorporated with cellulose, achieving satisfactory UV-protective properties.11–13 The UV protection factor (UPF) values of textiles can be increased by treating them with high concentrations of ZnO nanoparticles.8 However, the excessive use of nanoparticles can lead to ecological problems because the nanoparticles remain in effluent solutions.2 On the other hand, TiO2 and ZnO particles embedded into an organic matrix can photocatalyze the degradation of polymer,14 in which case the photostabilization of the hybrid structure is an additional requirement that must be taken into account.

Recently, Moraes et al. reported a UV-shielding composite film based on graphene oxide (GO) and cellulose acetate (CA) that possessed good absorbance of UV light at wavelengths between 250 nm and 350 nm.15 However, the mechanical strength was very low possibly due to the weak interaction between oxygen-containing groups on GO and ester groups on CA chains.

Aliphatic polyesters constitute the most versatile group of degradable polymers with good mechanical properties and good biocompatibility, and are particularly interesting as a promising matrix component in bionanocomposites. Currently, poly(ε-caprolactone) (PCL), produced by ring-opening polymerization (ROP) of cyclic ε-CL monomer,16–19 represents the most typical biodegradable and biobased polymer on the market owing to its cost-competitiveness compared with conventional non-biodegradable polymers.20 Cellulose-g-PCL has been used in many applications, such as self-assembled nanomicelles in drug delivery and surface-grafted cellulose nanocrystals for reinforcement.21,22 However, few monomers were attached to crystalline regions of cellulose in the heterogeneous synthesis process, owing to hydrogen bonds between the hydroxyl groups.23 Therefore, it is of great importance to obtain homogeneous cellulose-g-PCL with controlled molecular side-chains. However, it is considerably energy-consuming to do this in 1-butyl-3-methylimidazolium chloride (BmimCl) even at a temperature of 130 °C for 24 h.24 Moreover, the synthesis conditions in tetrabutylammonium fluoride (TBAF)/dimethyl sulfoxide (DMSO) are vague.25

In the present study, MCC-g-PCL was homogeneously prepared in tetrabutylammonium acetate (TBAA)/DMSO solvent at 60 °C (Fig. 1). And the MCC-g-PCL film was crosslinked using GO crosslinker under homogeneous conditions using DMSO as solvent. The structure, morphology and mechanical properties of the modified cellulose film were then studied. Finally, the protection of GO/MCC-g-PCL against UV light was investigated.


image file: c8ra00120k-f1.tif
Fig. 1 Scheme outlining the synthesis of MCC-g-PCL and the fabrication of GO/MCC-g-PCL hybrid films by solvent casting: (a) MCC film, (b) MCC-g-PCL film and (c) GO/MCC-g-PCL film.

2 Experimental

2.1 Materials

Avicel powder with a degree of polymerization of 200 was provided by Sinopharm Chemical Reagent Co., Ltd, PR China. The monomer ε-caprolactone with a purity of 99.9% used in the preparation of cellulose graft copolymers was obtained from Shandong Xiya Chemical Co., Ltd, PR China, and was used as received without any further purification. The tetrabutylammonium acetate (TBAA) (≥90.0%) and tetrabutylammonium fluoride hydrate (TBAF·3H2O) (≥98.0%) used as solvent for the cellulose solubilization were purchased from Tokyo Chemical Industry Co., Ltd, Japan. The dimethyl sulfoxide used as assistant solvent for the dissolution of cellulose was of analytical reagent grade and obtained from Beijing Chemical Works, PR China. 4-Dimethylaminopyridine (DMAP) and tin(II)ethylhexanoate of ≥95% and ≥99% purity, respectively, were supplied by Shanghai Macklin Biochemical Co., Ltd, PR China.

2.2 Preparation of microcrystalline cellulose-grafted polycaprolactone (MCC-g-PCL) and its composite materials

TBAA and DMSO were mixed in a mass ratio of 2[thin space (1/6-em)]:[thin space (1/6-em)]8 at 60 °C. Cellulose pulp was added slowly into the solvent medium. The mixture of cellulose/TBAA/DMSO was stirred at 60 °C for up to 30 min until a colorless solution was obtained. A solution of 13 mL ε-caprolactone containing 1.35 g DMAP was added to 20 g of 6 wt% cellulose solution. Polymerization was carried out for 24 h at 60 °C. After isolation, the polymer was washed and freeze-dried for 48 h.

After 105 mg GO was dispersed in 11.90 DMSO by ultrasonication for 12 h at room temperature, 2.10 g of the MCC-g-PCL prepared above was added and dissolved in the dispersion. Then GO/MCC-g-PCL composite film was prepared via the solvent immersion casting process and finally obtained after drying for 24 h in an air drying oven at 25 °C.

2.3 Structure characterization of MCC-g-PCL

The contents of grafted PCL in MCC-g-PCL copolymers were characterized by 1H nuclear magnetic resonance (NMR) spectroscopy. 1H NMR spectra were recorded at 400 MHz using a Bruker BioSpin NMR spectrometer (Bruker Company, Germany) in dimethyl sulfoxide-d6 (DMSO-d6) solvent. The chemical shifts were calibrated against the internal standard signals of tetramethysilane (TMS). 13C NMR spectra were acquired on a Bruker BioSpin NMR apparatus at 100 MHz, at ambient temperature, using TMS as the internal standard and DMSO-d6 as solvent.

Raman spectroscopy was conducted on a Renishaw InVia Reflex Raman system. The Raman scattering was excited using a diode laser at a wavelength of 785 nm. The laser beam was focused on the sample with a 100 an0.85 microscope objective. The laser power at the sample was 320 mW. The exposure was 10 s and two accumulations of Raman measurements were carried out. In addition, an optical microscope was coupled to the system.

The molecular weight and molecular weight distribution of prepared MCC-g-PCL were measured on a Waters 5510 gel permeation chromatograph (U.S.A.). DMSO was used as eluent at a flow rate of 0.5 mL min−1 at 50 °C. The SEC system was calibrated with linear polystyrene standards.

2.4 Characterization of GO/MCC-g-PCL composite film

The surface morphology of the nanocomposite films was examined using a scanning electron microscope (S-4800, Hitachi, Japan) operated at an accelerating voltage of 10 kV with a working distance of 20 mm. The films were cut into small pieces and fixed on conductive carbon tape. Moreover, the composite materials were immersed in liquid nitrogen and then fractured in order to analyze their cross-sections by scanning electron microscopy (SEM). The films were then sputtered with a thin layer of gold for 60 s with a sputter-coating unit.

Fourier transform infrared (FT-IR) spectra were collected with a VERTEX TOV spectrometer (Bruker, Germany), to determine the interfacial bonds in MCC and MCC-g-PCL. All spectra were recorded at 2 cm−1 resolution with 32 consecutive scans within the standard wavenumber range from 4000 to 400 cm−1. All the samples were dried under vacuum at 50 °C for 24 h before testing.

The thermal stability of MCC, MCC-g-PCL and GO/MCC-g-PCL films was tested with an STA 449 F3 Jupiter analyzer (NETZSCH, Germany). Samples were heated from 25 °C to 600 °C at a constant heating rate of 10 °C min−1. All the measurements were performed under a nitrogen atmosphere.

Ultraviolet-visible (UV-vis) spectroscopy was applied to study the UV-vis transmittance of MCC, MCC-g-PCL and GO/MCC-g-PCL films. For each sample, wavelength scanning was performed in three random places along the film. The wavelength was monitored from 200 to 800 nm, and spectra were taken on an Agilent/Varian Cary 5000 UV-vis spectrophotometer.

The tensile strength and elongation-at-break of the films were measured in a conditioned state at 25 °C, using a universal tensile testing machine (ZB-WL300, Hangzhou Zhibang Automated Instrument Co., Ltd, PR China) with crosshead speed of 5 mm min−1. The specimens, measuring 10 mm × 60 mm, were prepared and tested under ambient conditions. To minimize the experimental error, the tensile tests were carried out at 10 mm min−1 on ten individual films for each sample.

3 Results and discussion

3.1 Structure and molecular weight of MCC-g-PCL

The typical 13C NMR spectrum of MCC-g-PCL copolymer is shown in Fig. 2A. The methylene carbon signals of PCL can be observed at δ = 32.6 ppm, 33.9 ppm, 25.5 ppm, 24.5 ppm, 28.1 ppm, 61.2 ppm and 64.1 ppm, ascribed respectively to the carbons in the a, a′, b, c, d, e′ and e ring-opened caprolactone positions. MCC-g-PCL displayed typical signals for cellulose.26,27 At the same time, the strong signals in the region between 50 and 120 ppm were assigned mainly to the different carbons of cellulose (Fig. 2A). The carbon signals of the cellulose backbone appearing at δ = 100.9 ppm and 64.1 ppm were assigned to C1 and C6, respectively, in the anhydrous glucose units (AGU).28 Carbons C2, C3 and C5 show a cluster of resonances at 71.5–76.9 ppm in the cross-polarization magic angle spinning (CP/MAS) 13C NMR spectrum.29 Moreover, the signal corresponding to the overlap of C6 bearing a substituted OH group with the methylene carbon of PCL in the e position appears at δ = 61.2 ppm. The carbon signal at δ = 99.5 ppm belongs to the C1 adjacent to the C2 with substituted OH groups, indicating PCL grafts at multiple sites of AGU. Especially, the peak at 173.4 ppm, identified as the carbonyl carbon signal of the PCL segment (in the f position), confirms successful synthesis of MCC-g-PCL.30
image file: c8ra00120k-f2.tif
Fig. 2 (A) 13C NMR spectrum, (B) 1H NMR spectrum, (C) gel permeation chromatography trace of MCC-g-PCL, and (D) Raman spectra of MCC and MCC-g-PCL.

In the 1H NMR spectrum of cellulose-g-PCL copolymer (Fig. 2B), the methylene proton peaks of PCL can be observed at δ = 3.98 ppm (CH2O, e, repeating units), 3.38 ppm (CH2OH, e′, end unit), 2.27 ppm (COCH2, a′, end unit), 1.52 ppm (COCH2, a, repeating unit), 1.41 ppm (CH2, b, d), and 1.29 ppm (CH2, c).31 The resonance peaks derived from the protons of AGU of the cellulose backbone appear at δ = 4.47 ppm and 3.53 ppm, attributed to H1 and H5,6,2, respectively. Meanwhile, the signals at δ = 5.51 ppm, 5.37 ppm, and 4.35 ppm correspond to the protons of the residual hydroxyl groups of AGU. According to these assignments, the molecular factors of the graft copolymers, including DP, MS, DS and weight content of the PCL side-chain, where MS is the molar substitution of PCL, DS is the degree of substitution of PCL (e.g. the number of PCL side-chains per cellulose unit), DPPCL is the degree of polymerization of PCL, and WPCL is the weight content of PCL side-chains. According to these assignments, the molecular factors of the graft copolymers including the degree of substitution, degree of polymerization, the molar substitution, and the weight content of PCL side chains can be estimated according to previous study.21 The appearance of proton signals of caproyl groups in this spectrum, further confirmed that MCC-g-PCL copolymers were synthesized successfully.

Fourier transform (FT)-Raman spectra in the frequency region of 2000–200 cm−1 for MCC and MCC-g-PCL are shown in Fig. 2D. For both MCC and MCC-g-PCL, the characteristic Raman band at 1500–1200 cm−1 was assigned to C–H bending.30 Additionally, a strong peak located at 1095.5 cm−1 corresponded to the cellulose C–O ring stretching32,33 with an alternative assignment for the glycosidic linkage (C–O–C) mode.34,35 The peak located around 894.9 cm−1 was assigned to mixed modes (C–C–C, C–H–O) including angle bending.32 The presence of a Raman band at 1740 cm−1, corresponding to carbonyl groups, indicated that the ring-opened caprolactone was successfully introduced into cellulose–OH groups by esterification catalyzed by DMAP. These results confirm the success of the grafting procedure.

The molecular weight of MCC-g-PCL was measured using gel permeation chromatography (Fig. 2C). The determined molecular weight of MCC-g-PCL is significantly higher than the molecular weight of native cellulose, which may be due to functionalization. The data verify that the presented cellulose grafting is mild and does not result in pronounced degradation of the cellulose backbone.

3.2 Morphology of composite materials

To study the influence of GO on the microstructure of MCC-g-PCL, the nanocomposite films were investigated by field emission scanning electron microscopy (FE-SEM). It can be observed that the pure MCC-g-PCL film with some long voids exhibits a clean but rough surface (Fig. 3(A3)), showing weak interaction between the MCC-g-PCL molecules, owing to the decreased numbers of hydroxyl groups in the cellulose chains and the hindrance of the PCL side-chains. In comparison with the pure MCC-g-PCL film, a regular uniform network structure (Fig. 3(B1)) of GO/MCC-g-PCL nanohybrids is observed clearly, which is expected to enhance their mechanical properties. The results show that the uniform network benefited from the excellent dispersion of GO nanohybrids within the MCC-g-PCL matrix, which is much smoother than the pure MCC-g-PCL film (Fig. 3(B3)). Therefore, the GO oxygenated groups might be interacting with the PCL chains, providing good compatibility between the GO filler and the polymer.
image file: c8ra00120k-f3.tif
Fig. 3 Scanning electron micrographs of (A) MCC-g-PCL and (B) GO/MCC-g-PCL films.

3.3 Contact angle

Since the ultimate goal of this study is to disperse as finely as possible the prepared GO composite materials in a hydrophobic polyester matrix, contact angle measurements were used to estimate the change in hydrophobicity of the grafted substrates compared with unmodified MCC, and a distinct difference in hydrophobicity was observed (Fig. 4). As shown in Fig. 4, the contact angle increases from 39.6° for the pure MCC film to 87.3° for the MCC-g-PCL, namely the MCC-g-PCL displays a higher hydrophobic nature,36 because of the shielding of PCL chains grafted onto the OH-rich hydrophilic surface of MCC.37 It should be noted that addition of GO did not cause a reduction in hydrophobicity of the MCC-g-PCL-based film's surface; on the contrary, the contact angle of GO/MCC-g-PCL film increased a little. Hence, GO/MCC-g-PCL composite materials showed a more hydrophobic nature as the hydroxyls of the MCC-g-PCL interacted with that of GO. This can be understood in light of the apparent irregular roughness of the GO/MCC-g-PCL film compared with MCC-g-PCL, distinguished from the surface SEM images of GO/MCC-g-PCL film and MCC-g-PCL film (Fig. 4), which increased the contact angle. Another possible reason is that the hydroxyl groups in GO are mostly occupied owing to its interaction with MCC-g-PCL.38 And the results are in accordance with that of rGO/CNC hybrid fibers as well.39 Moreover, the addition of GO sheets also influenced the porosity and pore size distribution of the membrane, which had an effect on the hydrophobicity of the film as well.
image file: c8ra00120k-f4.tif
Fig. 4 Contact angles of (a) MCC, (b) MCC-g-PCL and (c) GO/MCC-g-PCL films.

3.4 FT-IR analysis

The FT-IR spectra of MCC, MCC-g-PCL and GO/MCC-g-PCL films are displayed in Fig. 5. Compared with the unmodified precursor, MCC film, MCC-g-PCL film showed a strong band at 1729 cm−1 which was assigned to the typical carbonyl group stretching. Other obvious transmittance bands located at about 2935 cm−1 and 2861 cm−1 correspond to C–H stretching of CH3 and CH2 groups, respectively. And the peak located at 1156 cm−1 is associated with C–H bending.40,41 FT-IR measurement also revealed the interactions between MCC-g-PCL matrix and GO filler. It seemed that the chemical surface composition of the composite films was not obviously affected by the introduction of GO but there were some differences. Compared with MCC-g-PCL film, the broadened peak at 3447 cm−1 and the relative intensity changes of the C–O stretching vibrations in the GO/MCC-g-PCL composites imply the disturbance of hydrogen-bonding in MCC-g-PCL, indicating the formation of intermolecular hydrogen bonds and excellent compatibility between GO and MCC-g-PCL.42–45
image file: c8ra00120k-f5.tif
Fig. 5 FT-IR spectra of (a) MCC, (b) MCC-g-PCL and (c) GO/MCC-g-PCL films.

3.5 Thermal stability

The thermogravimetric analysis (TGA) curves (Fig. 6) showed a one-step profile of weight loss for neat MCC, MCC-g-PCL and GO/MCC-g-PCL composites, which was related to the degradation of carbonyl groups and the chains of cellulose.46 It was observed that the polymer grafting improved the thermal stability of the film. Thermal degradation of neat MCC, which was due to depolymerization, dehydration and decomposition of cellulosic glycosyl units,47 started at 256 °C and reached its maximum value (Tmax) at 329 °C. Polymer-grafted MCC started to decompose at a temperature of approximately 205 °C, which was substantially lower than that of the pristine MCC sample. The MCC-g-PCL film displayed a slower degradation rate between 250 and 400 °C and a higher residual mass at high temperature compared with MCC. The enhanced thermal stability of MCC-g-PCL may originate from the entanglement of the PCL side-chains, which provided indirect confirmation of successful grafting of polymer brushes on MCC. It is clearly seen that the TGA curves of pure MCC-g-PCL and GO/MCC-g-PCL films are practically overlapping, indicating that the thermal decomposition behavior of GO/MCC-g-PCL is almost identical to that of neat MCC-g-PCL films, suggesting a strong interaction between GO sheets and MCC-g-PCL chains. This may be due to the effect of nanoclay on the polymer matrix, and was similar to the effect of GO on thermal properties of GO/cellulose and GO/chitosan films.48,49
image file: c8ra00120k-f6.tif
Fig. 6 Thermogravimetric analysis plots for (a) MCC, (b) MCC-g-PCL and (c) GO/MCC-g-PCL films.

3.6 Mechanical properties

The mechanical properties of MCC, MCC-g-PCL and the GO/MCC-g-PCL composite are compared in Table 1. Neat MCC film was stiff with a tensile strength of 9.63 MPa and a strain at breaking of 3.6%. As observed from the results of mechanical analysis, MCC-g-PCL exhibited poor tensile strength of 2.63 MPa and a higher elongation-at-break of 6.4% as compared with the pristine MCC film, which may be due to the inner plasticization effect of PCL side-chains. The GO/MCC-g-PCL film showed distinct improvement of the tensile strength compared with MCC-g-PCL film. The film with 1.0 wt% GO had a tensile strength of 4.55 MPa, which was enhanced by 73.0% compared with that of pure MCC-g-PCL (2.63 MPa), attributed to the increased intermolecular hydrogen-bonding between the hydroxyl groups of MCC-g-PCL and hydroxyl or carboxyl groups of GO. In addition, the MCC-g-PCL acted as glue and GO sheets acted as reinforcement, the two playing a coordinated role. This may be due to the improved interfacial strength between PCL side-chains and GO. The GO sheets present a bigger surface area which could provide greater geometric constraints for the randomness of polymer molecules,50 providing improved surface interlocking with the PCL matrix, which has already been confirmed from SEM micrographs. The elongation-at-break of GO/MCC-g-PCL was increased from 6.4% up to 15.5%, which was similar to the values for epoxy composites filled with both graphene oxide (GO) and diglycidyl ether of bisphenol-A functionalized GO (DGEBA-f-GO) sheets and regenerated cellulose/graphite oxide.51,52 This increase in elongation of the composites was related with the origin of GO platelet structure. On the other hand, it may be attributed to the excellent dispersion of GO, enhancing the interfacial adhesion provided by the grafted PCL chains.53,54 More precisely, it has been previously suggested that grafted chains create a co-continuous phase in which local stresses are evenly transferred to the remaining PCL phase, which in turn improves the mechanical properties of the bulk material.55 Further, the hydroxyl end-group on PCL grafted onto the MCC reacted with the carboxyl group of GO sheets, which significantly increased the adhesion at the interface. These results, combined with the fact that cellulose-based composite film containing GO provided better mechanical properties than neat MCC-g-PCL film, agree with those obtained by Han et al., who prepared cellulose/graphite oxide composite film to study its mechanical behavior.51
Table 1 Mechanical properties of composite films
Sample Tensile strength (MPa) Elongation-at-break (%) Contact angle (°)
MCC 9.53 ± 0.44 3.6 ± 0.33 39.6
MCC-g-PCL 2.63 ± 0.18 6.4 ± 0.29 93.7
GO/MCC-g-PCL 4.55 ± 0.15 15.5 ± 0.51 87.3


3.7 UV-vis transmittance

The light transmittance of MCC, MCC-g-PCL and GO/MCC-g-PCL composite films was measured using UV-vis spectroscopy, and the results are shown in Fig. 7. Pure MCC film exhibited light transmittance higher than 91% across the visible light range (400–800 nm), and it did not demonstrate an anti-UV property as it presented a transmittance of over 60% even at 200 nm. In contrast to the findings for CA film reported in a previous study,15 our results showed that cellulose grafted with polycaprolactone film without incorporation of GO had good ability to shield against UV light. Notably, the MCC-g-PCL film possessed good UV-shielding capacity at 200–400 nm compared with MCC films. Therefore, a novel material with enhanced light-shielding capacity and good optical transparency in the visible light range was obtained through the modification of MCC into MCC-g-PCL. GO/MCC-g-PCL composite films offered an improved high-energy light-shielding capacity as compared with MCC-g-PCL film, especially at 250–400 nm. Particularly for UVC irradiation (250 nm), the GO/MCC-g-PCL film containing 1.0 wt% GO displayed a UV-shielding capacity of 43.8%, combined with 70.2% optical transparency under visible light. These results are in accordance with a previous study which reported that cellulose films showed reduced optical transmittance (from 91.5% to 78.2%) after blending with 0.4 wt% grapheme,56 revealing an effective anti-UV property with comparable transparency, which was competitive with transparent cellulose nanocrystals (CNC)/polylactic acid (PLA) and GO/cellulose acetate (CA) films,15,57 especially at wavelengths between 300 and 400 nm. In addition, although surface-functionalized zirconia nanoparticles/poly(butanediol monoacrylate) films had better UV-shielding capacity than the GO/MCC-g-PCL film prepared in the present study, their transmittance of visible light was very low.58
image file: c8ra00120k-f7.tif
Fig. 7 UV-vis spectra of (a) MCC, (b) MCC-g-PCL and (c) GO/MCC-g-PCL hybrid films.

4 Conclusions

In the present study, we demonstrated an efficient method for the facile preparation of MCC-g-PCL in a TBAA/DMSO solvent system in conjunction with ε-caprolactone, and characterized the structure and molecular weight. Furthermore, we also demonstrated an easy method of preparing a biocomposite from MCC-g-PCL and GO that served as a good example of ultraviolet-shielding, and was more environmental friendly. The GO introduced into the composite remarkably influenced both the inherent structure of the MCC-g-PCL and the surface morphology of the film. Moreover, the GO/MCC-g-PCL composite showed significantly improved mechanical properties compared with those of the pure MCC-g-PCL film, owing to the strong hydrogen-bonding interaction that physically crosslinked GO with MCC-g-PCL, while no changes of thermal stability were found. Moreover, GO/MCC-g-PCL composite films containing 1.0 wt% GO offered an effective high-energy light-shielding capacity for light between 200 nm and 300 nm in wavelength. This technique may lead to new and convenient methods for the production of various modified forms of cellulose and the processing of new composite materials from previously incompatible components.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

The authors are grateful for the support of the Project of Scientific Research Special Fund for Public Industry in Forestry (201504602-2).

Notes and references

  1. A. Gao, C. Zhang, K. Song and A. Hou, Carbohydr. Polym., 2014, 114, 392–398 CrossRef CAS PubMed.
  2. M. Gorjanc, K. Jazbec, M. Šala, R. Zaplotnik, A. Vesel and M. Mozetič, Cellulose, 2014, 21(4), 3007–3021 CrossRef CAS.
  3. K. Jazbec, M. Šala, M. Mozetič, A. Vesel and M. Gorjanc, J. Nanomater., 2015, 16(1), 1–9 Search PubMed.
  4. D. Zhang, L. Chen, D. Fang, G. William Toh, X. Yue, Y. Chen and H. Lin, Text. Res. J., 2013, 83(15), 1625–1633 CrossRef.
  5. J. D'Orazio, S. Jarrett, A. Amaro-Ortiz and T. Scott, Int. J. Mol. Sci., 2013, 14(6), 12222–12248 CrossRef PubMed.
  6. N. Deeba, I. Mohammad, S. Maria and M. Hasan, Curr. Drug Targets, 2013, 14(10), 1128–1134 CrossRef.
  7. M. Montazer and A. Maali, J. Phys. Chem. B, 2014, 118(6), 1453–1470 CrossRef CAS PubMed.
  8. W. Sricharussin, P. Threepopnatkul and N. Neamjan, Fibers Polym., 2011, 12(8), 1037–1041 CrossRef CAS.
  9. L. Xu, G. Zheng, J. Miao and F. Xian, Appl. Surf. Sci., 2012, 258(19), 7760–7765 CrossRef CAS.
  10. M. Montazer, M. Amiri and M. Malek, Photochem. Photobiol., 2013, 89(5), 1057–1063 CrossRef CAS PubMed.
  11. A. Becheri, M. Dürr, P. Nostro and P. Baglioni, J. Nanopart. Res., 2008, 10(4), 679–689 CrossRef CAS.
  12. Ş. Uğur, M. Sarıışık, H. Aktaş, Ç. Uçar and E. Erden, Nanoscale Res. Lett., 2010, 5(7), 1204 CrossRef PubMed.
  13. A. Yadav, V. Prasad, A. Kathe, S. Raj, D. Yadav, C. Sundaramoorthy and N. Vigneshwaran, Bull. Mater. Sci., 2006, 29(6), 641–645 CrossRef CAS.
  14. R. Yang, P. Christensen, T. Egerton and J. White, Polym. Degrad. Stab., 2010, 95(9), 1533–1541 CrossRef CAS.
  15. A. C. de Moraes, P. F. Andrade, A. F. de Faria, M. B. Simoes, F. C. Salomao, E. B. Barros, C. Goncalves Mdo and O. L. Alves, Carbohydr. Polym., 2015, 123, 217–227 CrossRef PubMed.
  16. Y. Teramoto, M. Yoshioka, N. Shiraishi and Y. Nishio, J. Appl. Polym. Sci., 2002, 84(14), 2621–2628 CrossRef CAS.
  17. Y. Teramoto and Y. Nishio, Polymer, 2003, 44(9), 2701–2709 CrossRef CAS.
  18. R. Shi and H. Burt, J. Appl. Polym. Sci., 2002, 89, 718–727 CrossRef.
  19. N. Lin, G. Chen, J. Huang, A. Dufrense and P. R. Chang, J. Appl. Polym. Sci., 2009, 113(5), 3417–3425 CrossRef CAS.
  20. A. Mujica-Garcia, S. Hooshmand, M. Skrifvars, J. M. Kenny, K. Oksman and L. Peponi, RSC Adv., 2016, 6, 9221–9231 RSC.
  21. Y. Guo, X. Wang, Z. Shen, X. Shu and R. Sun, Carbohydr. Polym., 2013, 92, 77–83 CrossRef CAS PubMed.
  22. Y. Habibi, A. Goffin, N. Schiltz, E. Duquesne, P. Dubois and A. Dufresne, J. Mater. Chem., 2008, 18, 5002 RSC.
  23. K. Beyaz, M. Charton, A. Rouilly, E. Vedrenne, C. Vaca-Garcia, A. Benaboura and S. Thiebaud-Roux, Ind. Crops Prod., 2017, 97, 32–40 CrossRef CAS.
  24. L. Xu, X. Lu and X. Cheng, RSC Adv., 2015, 5, 79022–79030 RSC.
  25. I. Ikeda, K. Washino and Y. Maeda, Sen'i Gakkaishi, 2003, 59(3), 110–114 CrossRef CAS.
  26. M. Ibrahim, W. El-Zawawy and M. Nassar, Carbohydr. Polym., 2010, 79, 694–699 CrossRef CAS.
  27. N. Lin, J. Huang, P. Chang, J. Feng and J. Yu, Carbohydr. Polym., 2011, 83, 1834–1842 CrossRef CAS.
  28. C. Yan, J. Zhang, Y. Lv, J. Yu, J. Wu, J. Zhang and J. He, Biomacromolecules, 2009, 10(8), 2013–2018 CrossRef CAS PubMed.
  29. H. Kono, S. Yunoki, T. Shikano, M. Fujiwara, T. Erata and M. Takai, J. Am. Chem. Soc., 2002, 124, 7506–7511 CrossRef CAS PubMed.
  30. A. Mayumi, T. Kitaoka and H. Wariishi, J. Appl. Polym. Sci., 2006, 102(5), 4358–4364 CrossRef CAS.
  31. C. Jiang, X. Wang, P. Sun and C. Yang, Int. J. Biol. Macromol., 2011, 48(1), 210–214 CrossRef CAS PubMed.
  32. R. Atalla and S. Nagel, Science, 1974, 185, 522–523 CAS.
  33. K. Kong and S. J. Eichhorn, J. Macromol. Sci., Part B: Phys., 2005, 44, 1123–1136 CrossRef CAS.
  34. N. Wanasekara, A. Michud, C. Zhu, S. Rahatekar, H. Sixta and S. Eichhorn, Polymer, 2016, 99, 222–230 CrossRef CAS.
  35. H. Edwards, D. Farwell and D. Webster, Spectrochim. Acta, Part A, 1997, 53, 2383–2392 CrossRef.
  36. H. Youssef, G. Anne-Lise, S. Nancy, D. Emmanuel, D. Philippe and D. Alain, J. Mater. Chem., 2008, 18(41), 5002–5010 RSC.
  37. G. Chen, A. Dufresne, J. Huang and P. Chang, Macromol. Mater. Eng., 2009, 294(1), 59–67 CrossRef CAS.
  38. R. Faradilla, G. Lee, J. Roberts, P. Martens, M. Stenzel and J. Arcot, Cellulose, 2018, 25(1), 399–416 CrossRef CAS.
  39. G. Chen, T. Chen, K. Hou, W. Ma, M. Tebyetekerwa, Y. Cheng, W. Weng and M. Zhu, Carbon, 2018, 127, 218–227 CrossRef CAS.
  40. H. Dong, Q. Xu, Y. Li, S. Mo, S. Cai and L. Liu, Colloids Surf., B, 2008, 66(1), 26–33 CrossRef CAS PubMed.
  41. Q. Xu, J. Kennedy and L. Liu, Carbohydr. Polym., 2008, 72(1), 113–121 CrossRef CAS.
  42. S. Gan, S. Zakaria and S. Jaafar, Carbohydr. Polym., 2017, 172, 284–293 CrossRef CAS PubMed.
  43. T. Kondo, J. Polym. Sci., Part B: Polym. Phys., 1994, 32(7), 1229–1236 CrossRef CAS.
  44. Y. Feng, X. Zhang, Y. Shen, K. Yoshinoc and W. Feng, Carbohydr. Polym., 2012, 87(1), 644–649 CrossRef CAS.
  45. L. Yao, Y. Lu, Y. Wang and L. Hu, Carbon, 2014, 69, 552–562 CrossRef CAS.
  46. A. de Oliveira, M. Ferrarezi, I. Yoshida and M. Goncalves, J. Appl. Polym. Sci., 2012, 123(4), 2027–2035 CrossRef.
  47. M. Roman and W. Winter, Biomacromolecules, 2004, 5, 1671–1677 CrossRef CAS PubMed.
  48. X. Zhang, X. Liu, W. Zheng and J. Zhu, Carbohydr. Polym., 2012, 88(1), 26–30 CrossRef CAS.
  49. D. Han, L. Yan, W. Chen and W. Li, Carbohydr. Polym., 2011, 83(2), 653–658 CrossRef CAS.
  50. Y. Pan, T. Wu, H. Bao and L. Li, Carbohydr. Polym., 2011, 83(4), 1908–1915 CrossRef CAS.
  51. D. Han, L. Yan, W. Chen, W. Li and P. Bangal, Carbohydr. Polym., 2011, 83(2), 966–972 CrossRef CAS.
  52. Y. Wan, L. Tang, L. Gong, D. Yan, Y. Li, L. Wu, J. Jiang and G. Lai, Carbon, 2014, 69, 467–480 CrossRef CAS.
  53. H. Lönnberg, K. Larsson, T. Lindström, A. Hult and E. Malmström, ACS Appl. Mater. Interfaces, 2011, 3(5), 1426–1433 Search PubMed.
  54. N. Lin, G. Chen, J. Huang, A. Dufrense and P. R. Chang, J. Appl. Polym. Sci., 2009, 113(5), 3417–3425 CrossRef CAS.
  55. X. Cao, Y. Habibi and L. Lucia, J. Mater. Chem., 2009, 19, 7137–7145 RSC.
  56. X. Zhang, X. Liu, W. Zheng and J. Zhu, Carbohydr. Polym., 2012, 88(1), 26–30 CrossRef CAS.
  57. J. Gwon, H. Cho, S. Chun, S. Lee, Q. Wu and S. Lee, RSC Adv., 2016, 6, 9438–9445 RSC.
  58. S. Scholz and S. Kaskel, J. Colloid Interface Sci., 2008, 323(1), 84–91 CrossRef CAS PubMed.

This journal is © The Royal Society of Chemistry 2018