Zhu-Bao Shaoa, Ming-Xin Zhanga, Ye Han*a, Xu-Dong Yanga, Jing Jina and Rong-Kun Jian*b
aInstitute of Chemical Engineering, Changchun University of Technology, Changchun 130012, China. E-mail: zhu871227@163.com
bFujian Key Laboratory of Polymer Materials, College of Materials Science and Engineering, Fujian Normal University, Fuzhou 350007, China. E-mail: jrkht1987@fjnu.edu.cn

Received 5th September 2017 , Accepted 20th October 2017

First published on 8th November 2017


Abstract

Traditional phosphorus–nitrogen (P–N) flame-retardant systems for polypropylene (PP) always act through joint action of the gaseous phase and condensed phase, and are accompanied with a decrease of the thermal stability and water resistance. In this work, a novel mono-component and gas-dominated flame retardant, named DPPIP, was prepared through an amidation reaction of diphenylphosphinyl chloride and piperazine, and used to flame retard PP. Experimental results confirmed that both the thermal stability and water resistance of PP/DPPIP were improved. The initial thermal decomposition temperature of PP/25 wt% DPPIP at 5 wt% weight loss was 287.5 °C under air atmosphere, which is higher than that of neat PP (266.1 °C). Besides, a water-resistance test verified that PP/25 wt% DPPIP had a weight loss of only about 0.52 wt%. More importantly, the flame retardant ability of PP/25 wt% DPPIP had been greatly improved, passing the V-0 rating (UL-94). Furthermore, after the water-resistance test, the LOI value of PP/25 wt% DPPIP exhibited nearly no difference and still passed the UL-94 V-0 rating. A cone calorimeter (CC) result indicated that DPPIP had a positive effect on inhibiting heat release of PP during combustion. All of these combustion tests displayed that there was no char left. The flame retardant mechanism of DPPIP was investigated with py-GC/MS and TG-FTIR. The results illustrated that the gaseous phase resulting from the thermal decomposition of DPPIP played the leading role in the self-extinguishing behavior of PP/DPPIP, which consisted of a large amount of inflammable gaseous products such as piperazine and its derivatives, and phosphorus-containing structures.


1. Introduction

Halogen-free flame retardant systems, such as metal hydroxides, metal borates and intumescent flame retardants (IFR) etc., have been utilized to obtain flame-retardant PP composites.1–4 Among these halogen-free flame retardant systems, intumescent flame retardants, especially phosphorus–nitrogen (P–N) flame retardants, have attracted much attention in flame-retardant PP due to their high flame-retardant efficiency.5–7

In order to obtain better flame-retardant efficiency of PP, a lot of work has been done in past decades, especially research on the flame-retardant mechanism. Generally, traditional P–N flame retardants for PP mainly contain three components, which are an acid source, blowing agent and charring agent,8,9 and when P–N flame retardants are heated beyond a critical temperature they can generate multicellular swollen chars on the surface of the polymer accompanied by decomposition of the blowing agent, slowing down the heat and oxygen transfer, thus protecting the substrate from burning.10,11 Therefore, these flame-retardant systems for PP usually act through a gaseous phase and condensed-phase flame-retardant mechanism together. Compared with the production of gas, the condensed-phase formation of P–O–C structures during combustion is one of the methods to improve the flame-retardant efficiency, and the typical flame retardant system is a mixture of ammonium polyphosphate and charring agent (CA).12–14 Wang et al.15 synthesized a novel charring agent (CA), namely MTEC, and found that a PP/APP/MTEC system could achieve a LOI value of 28.5% and acquire a UL-94 V-0 rating at 20 wt% APP/CA through the formation of P–O–C structures during combustion. The condensed-phase formation of P–N–C structures during combustion is also an efficient method to enhance the flame-retardant efficiency of PP. In our previous papers,16–18 APPs modified with ethylenediamine (EDA), ethanolamine (ETA) or piperazine (PIP) were incorporated alone into PP. The results also indicated that P–N–C structures were formed during combustion, which could enhance the flame-retardant efficiency for PP. In summary, APP is an essential component to facilitate the formation of stable char during two P–N flame-retardant methods. Unfortunately, the thermal stability and water resistance of APP and modified APPs were not improved due to the production of large amounts of amine salts and the introduction of organic amine salts. Although lots of work has been done, such as the modification of APP and microencapsulated APP,13,19 these problems still exist, which has limited the application of APP in the practical field. Thus, some researchers have considered whether PP could obtain an excellent efficiency only acting through a gas-dominated flame retardant.

In the present work, a novel mono-component, only gas-dominated and P–N containing flame retardant, named DPPIP, was synthesized through the reaction of diphenylphosphinyl chloride and piperazine, and different measurements were used to confirm its chemical structure. The thermal stability and water resistance of DPPIP were examined. PP/DPPIP blends were prepared via physical blending, and their thermal stability, water-solubility and flame retardancy were also studied. Finally, the flame retardant mechanism of DPPIP was investigated with the aid of different measurements.

2. Experimental section

2.1. Materials

Diphenylphosphinyl chloride (DPPC) was supplied by Shanghai Changgen Chemical Reagent Co., Ltd. (Shanghai, China); piperazine (AR), chloroform (AR) and triethylamine (AR) were purchased from Tianjin Kemiou Chemical Reagent Co., Ltd. (Tianjin, China); polypropylene (T30S) was obtained from Petro China Lanzhou Petrochemical Co., Ltd. (Lanzhou, China).

2.2. Measurements

Fourier transform infrared spectroscopy (FTIR) tests were performed on a Nicolet FTIR 170SX spectrometer (Nicolet, America) using a KBr disk, and the wavenumber range was set from 4000–400 cm−1.

1H nuclear magnetic resonance (1H-NMR) spectra and 31P nuclear magnetic resonance (31P-NMR) spectra were recorded on a Bruker AV II-400 MHz spectrometer (Bruker, Switzerland) using CDCl3 as solvent. The sample (85 mg) was put into an NMR tube, then a solution of CDCl3 (5 mL) was injected into the NMR tube, and next the NMR tube was shaken until the solids were dissolved in CDCl3. The concentrations of DPPIP, PIP or DPPC were about 1.7 g/100 mL. The NMR test was performed at about 25 °C, and TMS was applied. The peak which appeared at 0 ppm in the 1H-NMR spectra was ascribed to TMS.

X-ray photoelectron spectroscopy (XPS) spectra were recorded on an XSAM80 spectrometer (Kratos Co, UK) equipped with Al Kα excitation radiation (-1486.6 eV).

Tensile testing was completed in accordance with the procedures in GB/T 1040.1-2006 at a crosshead speed of 20 mm min−1. The Izod impact properties were tested in accordance with the procedures in GB/T 1843-2008 and the depth of the nick was 2 mm.

Thermogravimetric (TG) analysis was carried out on a TG 209 F1 (NETZSCH, Germany) thermogravimetric analyzer at a heating rate of 10 °C min−1 under a nitrogen or air flow of 50 mL min−1 in the temperature range from 40 to 700 °C.

The LOI value was measured using an HC-2C oxygen index instrument (Jiangning, China) according to ASTM D2863-97. The sheet dimensions of all of the samples were 130 mm × 6.5 mm × 3.2 mm.

The UL-94 vertical burning level was tested on a CZF-2 instrument (Jiangning, China) according to ASTM D 3801. The dimensions of the samples were 130 mm × 13 mm × 3.2 mm.

The flammability of the samples was measured on a CC device (Fire Testing Technology, UK). Samples with dimensions of 100 mm × 100 mm × 3 mm were exposed to a radiant cone at a heat flux of 50 kW m−2.

The thermogravimetry-Fourier transform infrared spectroscopy (TG-FTIR) apparatus consisted of a TG 209 F1 (NETZSCH, Germany) thermogravimetric analyzer and a 170 SX FTIR spectrometer (Nicolet, America). A sample (about 6 mg) was heated at a rate of 10 °C min−1 in the temperature range from 40 to 700 °C under a nitrogen flow of 50 mL min−1.

The samples for the py-GC/MS tests were first pyrolyzed in a pyrolyzer (CDS5200) under helium atmosphere. The relevant samples (300 μg) were heated from ambient temperature to 600 °C at a rate of 20 °C ms−1 and kept for 15 s. Then, the volatile products were carried through helium to a Perkin-Elmer Clarus680GC-SQ8MS system coupled with the pyrolyzer. The temperature of the capillary column (HP-5, 0.25 mm) of the GC was held at 40 °C for 3 min; afterward, the temperature was increased to 280 °C at a heating rate of 10 °C min−1 and then kept at 280 °C for 5 min. The injector temperature was maintained at 280 °C. The MS indicator was operated in the electron impact mode at an electron energy of 70 eV, and the ion source temperature was kept at 250 °C. The identification of the pyrolysis products was carried out by comparing to the NIST MS library.

The water-resistance of the flame retardant and modified PP was tested according to the following procedure: 10 g of flame retardant was put into 100 mL of distilled water at 70 °C and stirred for 60 min. The suspension was then filtered. Next, the obtained solid was dried to a constant weight at 100 °C. Finally, the solubility of the flame retardant in water was obtained.20 The modified PP (the weight of M0) was put into distilled water at 70 °C, and kept at this temperature for 168 h (the water was replaced at each interval of 24 h). Then the treated specimens were taken out, and dried to a constant weight at 100 °C. The weight of the dried sample is M1, so the weight loss can be calculated based on the following equation: [(M0M1)/M0] × 100%.20

2.3. Synthesis of DPPIP

47 g of diphenylphosphinyl chloride and 100 mL of chloroform were mixed in a 250 mL three-necked round-bottom flask equipped with a reflux condenser, dry N2 inlet, and a dropping funnel. The mixture was agitated in an ice-bath under nitrogen atmosphere. Half an hour later, 8 g of piperazine dissolved in chloroform (20 mL) was added over 1 h. Then 60 g of triethylamine was added to the solution. After completing the addition, the solution was heated to 75 °C for 8 h until the reaction completely finished. Finally, the solution was cooled to room temperature and then filtered. The filtrate was evaporated under reduced pressure to obtain the crude product. The product was washed with water repeatedly to remove the impurities, then dried at 85 °C for 12 h under vacuum to a constant weight (84.3% yield). The reaction formula is described in Scheme 1.
image file: c7ra09868e-s1.tif
Scheme 1 The synthetic route of DPPIP.

2.4. Sample preparation

DCPIP was dried in a vacuum oven at 85 °C for 12 h. Then PP blends filled with different ratios of DCPIP were prepared via a twin-screw extruder (CTE 20, Kebeilong Keya Nanjing Machinery Co., Ltd, Nanjing, China) with a rotation speed of 150 rpm with the following temperature protocol from the feed zone to the die: 175, 180, 190, 185, 180 and 170 °C. Finally, the extruded pellets were hot-pressed into different samples by a plate vulcanizer (Qingdao Yadong Rubber Viachinery Co. Ltd. China).

3. Results and discussion

3.1. Characterization of DPPIP

The FTIR spectrum of DPPIP is shown in Fig. 1. The peaks at around 3025.6–3059.4 cm−1 and 760.9 cm−1 are ascribed to the C–H vibrations of the benzene rings. The peaks located at 2948.6–2962.8 cm−1 are assigned to the C–H stretching vibrations of PIP. The peaks at 1116.4 cm−1 and 722.5 cm−1 correspond to the P–N–C vibrations,16–18 and the peak at 1178.8 cm−1 is assigned to the P[double bond, length as m-dash]O vibration. The results show that DPPIP had been prepared successfully.
image file: c7ra09868e-f1.tif
Fig. 1 FTIR spectrum of DPPIP.

To confirm the formation of DPPIP, 1H-NMR and 31P-NMR tests of DPPC, PIP and DPPIP were performed, and the results are displayed in Fig. 2. All of the protons can be attributed to the expected signals. Compared with the 1H-NMR spectrum of PIP (Fig. 2b), the N–H signal at 1.75 ppm disappeared and the peak at 2.80 ppm shifted to 3.11 ppm in DPPIP, which is assigned to –CH2– in the –CH2–N–P– group, indicating that the P–N bond is formed. In the 31P-NMR spectra, there was only one peak at 44.95 ppm for DPPC, which is ascribed to the P in the –P–Cl group, and DPPIP displayed one characteristic peak at 29.47 ppm, indicating that the P–N bond is formed and a high purity of DPPIP. All of the 1H-NMR and 31P-NMR results demonstrate that DPPIP was obtained successfully.


image file: c7ra09868e-f2.tif
Fig. 2 1H-NMR and 31P-NMR spectra of DPPC (a), PIP (b) and DPPIP (c).

To further determine the structure of DPPIP, XPS measurements of PIP and DPPIP were carried out. Their N1s spectra are shown in Fig. 3. For PIP, the peak at 399.2 eV is ascribed to the N in –C–NH–C–.17 While for DPPIP, a new peak at 402.0 eV is attributed to the N in –P–N–C–, further indicating that DPPIP was formed.


image file: c7ra09868e-f3.tif
Fig. 3 N1s spectra of PIP (a) and DPPIP (b).

3.2. Water resistance

Water resistance is an important property to assess the usability of flame retardants in polymers. Thus, the water solubility of DPPIP was tested and compared with our previously modified APPs (PA-APP), and the corresponding data are listed in Table 1. It could be observed that PA-APP is easily dissolved in 70 °C water due to the large amount of hydrophilic amine salt, and the water solubility value is 10.0 g/100 mL of water. However, because of the hydrophobic nature of P–N and the benzene rings, the water solubility of DPPIP is less than 0.01 g/100 mL of water. Moreover, the water resistance of PP/DPPIP and PP/PA-APP was also evaluated through water-solubility experiments, and the results are listed in Table 1. For PP/DPPIP, the weight loss is only 0.52 wt%, which is far less than that for PP/PA-APP. These results demonstrate that DPPIP and PP/DPPIP have an excellent water resistance.
Table 1 Water solubility of DPPIP, PA-APP, PP/DPPIP and PP/PA-APP
Sample Average water solubility (g/100 mL of water) Sample Average weight loss (wt%)
DPPIP <0.01 PP/25 wt% DPPIP 0.52 ± 0.02
PA-APP =10.0 PP/25 wt% PA-APP 6.53 ± 0.04


3.3. Thermogravimetric analysis

TG and derivative thermogravimetric (DTG) curves of neat PP, DPPIP and PP/DPPIP under N2 and air atmosphere are illustrated in Fig. 4, and the corresponding data are listed in Table 2. There is only one degradation step for DPPIP ranging from 300–420 °C under N2 atmosphere, and the initial decomposition temperature (T5%, defined as the temperature where the mass loss is 5 wt%) of DPPIP is 328.9 °C, which is lower than that of neat PP (383.5 °C). Consequently, with the addition of DPPIP, the initial decomposition temperature of modified PP (N2) decreased, and it corresponds well to that in the calculated curve. However, the degradation of PP/DPPIP under air atmosphere is very different, as the initial decomposition temperature of DPPIP (310.8 °C) is higher than that of neat PP (266.1 °C). As shown in Fig. 4c and d, with the temperature rising, the residues at 700 °C are almost gone for the neat PP, DPPIP and PP/DPPIP both under N2 and air atmosphere. The TG results suggest that the char layer is not formed at 700 °C, indicating that DPPIP generated almost only gas-phase products during the decomposition.
Table 2 Thermogravimetric properties of PP, DPPIP and PP/DPPIP
Sample N2 Air
T5% (°C) Tmax (°C) Residue (%) T5% (°C) Tmax (°C) Residue (%)
1 2 1 2
Neat PP 383.5 451.9 0.0 266.1 338.4 0.0
DPPIP 328.9 416.3 0.0 310.8 387.3 0.1
PP/25 wt% DPPIP 340.1 404.6 451.0 0.0 287.5 332.1 398.2 0.1
Calculated data 368.0 422.5 452.5 0.0 268.5 340.1 387.5 0.0



image file: c7ra09868e-f4.tif
Fig. 4 TG and DTG curves of neat PP, DPPIP, and PP/25 wt% DPPIP and the calculated curve of PP/25 wt% DPPIP at a heating rate of 10 °C min−1 under N2 (a, b) and air (c, d) atmosphere.

3.4. Mechanical properties of flame-retardant PP composites

The mechanical properties of PP/PA-APP and PP/DPPIP, including the tensile strength, elongation at break, and impact strength, are listed in Table 3. Compared with PP/PA-APP, PP/DPPIP with an equal amount of flame retardant had no apparent change in the impact strength, but both the tensile strength and elongation at break for PP/DPPIP increased. Therefore, it can be concluded that DPPIP is more conducive to the improvement of the mechanical properties of flame-retardant PP than PA-APP.
Table 3 Mechanical properties of PP/DPPIP and PP/PA-APP
Sample Flame retardant (wt%) Tensile strength (MPa) Elongation at break (%) Impact strength (kJ m−2)
PP/DPPIP 20 38.8 ± 0.3 113.3 ± 5.4 1.83 ± 0.04
25 33.2 ± 0.2 87.5 ± 6.3 1.95 ± 0.03
30 29.5 ± 0.3 60.4 ± 4.5 1.98 ± 0.04
PP/PA-APP17 20 33.0 ± 0.4 92.4 ± 8.2 1.85 ± 0.02
25 30.6 ± 0.3 80.7 ± 5.4 1.92 ± 0.03
30 25.2 ± 0.2 43.2 ± 5.5 2.02 ± 0.03


3.5. Flame retardancy

The flame retardant performances of neat PP and PP/DPPIP before and after water-resistance tests were evaluated by LOI and UL-94 testing, and the corresponding data are listed in Table 4. The two tests showed that neat PP is a flammable polymer. For PP/DPPIP, with an increasing amount of DPPIP, the LOI value increased from 18.0% (neat PP) to as high as 28.5% with the addition of 30 wt%. Furthermore, with only 25 wt% addition of DPPIP, the flame-retardant PP can pass the UL-94 V0 rating and dripping is not observed. After the water treatment, the LOI value of flame-retardant PP decreased slightly, and when the addition of DPPIP was 25 wt%, the LOI value decreased from 27.0% to 26.9%, and this can still pass the UL-94 V0 rating. These results indicate that DPPIP is an effective flame retardant for PP, which could further meet the needs of practical application.
Table 4 LOI and UL-94 results of neat PP and PP/DPPIP before and after water resistance testing
Component (wt%) Not treated with water After water treatment
LOI (%) UL-94 (3.2 mm) LOI (%) UL-94 (3.2 mm)
PP DPPIP Rating Dripping Rating Dripping
100 0 18.0 NR Yes
80 20 24.5 NR Yes
75 25 27.0 V0 No 26.9 V0 No
70 30 28.5 V0 No


CC testing is an effective method to assess the combustion behavior of materials. The corresponding heat release rate (HRR), total heat release (THR), smoke production rate (SPR) and total smoke production (TSP) curves of neat PP and PP/25 wt% DPPIP are shown in Fig. 5 and 6, and the corresponding data are presented in Table 5. As shown in Table 5, the time to ignition (TTI) of the neat PP (20 s) is far lower than that of PP/DPPIP (58 s) due to the early decomposition of neat PP at the beginning of combustion, which is in accordance with the TGA results in air atmosphere. Therefore, the ignition-resistance of the composite is improved. With the addition of DPPIP, both the peak of the HRR (PHRR) and the THR of PP/25 wt% DPPIP decreased compared with those of neat PP, especially for the PHRR, which decreased from 904.4 kW m−2 to 487.7 kW m−2 with a reduction of 46.1% compared with that of PP, indicating that the presence of DPPIP is favorable to suppress the heat release of neat PP.


image file: c7ra09868e-f5.tif
Fig. 5 HRR (a) and THR (b) plots of PP/25 wt% DPPIP.

image file: c7ra09868e-f6.tif
Fig. 6 SPR (a) and TSP (b) plots of PP/25 wt% DPPIP.
Table 5 CC data of neat PP and PP/25 wt% DPPIP composites
Sample Neat PP PP/DPPIP
TTI (s) 20 58
Peak HRR (kW m−2) 904.4 487.7
Time to PHRR (s) 140 135
FGR (kW m−2 s) 6.46 3.61
THR (MJ m−2) 126.2 87.5
Char residue (wt%) 0.5 1.1


Based on the HRR curves, the fire growth rate (FGR) has been calculated to assess the fire hazard of the composite according to the following equation:21,22

FGR = PHRR/tPHRR

Generally, a lower FGR value indicates that the time to flashover is delayed.21 For PP/DPPIP, the FGR decreased from 6.46 kW m−2 s to 3.61 kW m−2 s, which was decreased by 44.1% compared with that of neat PP. This result suggests that the introduction of DPPIP could significantly reduce the FGR of the PP composite, and consequently could significantly extend the time to escape in a real incident.

The SPR and TSP curves of neat PP and PP/DPPIP are presented in Fig. 6, and the corresponding data are summarized in Table 5. It is clear that the SPR and TSP of PP/DPPIP increased more significantly compared with those of neat PP. The results illustrate that PP/DPPIP could produce lots of smoke, and suggest that DPPIP generates gas-phase products during the decomposition.

The digital photos of the residues for neat PP and PP/DPPIP after the CC test are shown in Fig. 7, and the char residues are listed in Table 5. There is almost nothing left after burning, which is in accordance with the TGA results in air and N2 atmosphere, indicating that the gaseous phase production from the decomposition of DPPIP plays a positive role in the flame retardancy of PP. This can be described as follows: during combustion the decomposition of DPPIP occurs, then a lot of inflammable gas is produced which could dilute the oxygen concentration. As a consequence, the formation of inflammable gas should be the most important factor to achieve a better flame retardancy of PP.


image file: c7ra09868e-f7.tif
Fig. 7 Digital photographs of residues of neat PP (a) and PP/25 wt% DPPIP (b) composites after the CC test.

3.6. The flame retardant mechanism of DPPIP

As mentioned above, to reveal the flame-retardant mechanism of DPPIP, the gaseous-phase activity of DPPIP is suggested. Thus, the gaseous phase products of DPPIP were investigated through TG-FTIR, and the FTIR spectra of the gaseous phase products of DPPIP during the thermal decomposition process under N2 atmosphere are shown in Fig. 8. The absorption peaks of the benzene rings at 3063.3 cm−1 and 695.1 cm−1 appeared at 328 °C, and some nitrogen-containing and carbon–hydrogen-containing products were released at 328 °C, as they presented the relevant characteristic absorption peaks at 2951.2 cm−1 (–CH–, –CH2–, –CH3) and 1437.6 cm−1 (–NH–, –NH2). Meanwhile, the absorption peaks at 1246.2 cm−1 (P[double bond, length as m-dash]O), 1125.2 cm−1 and 960.6 cm−1 (P–C) and 1125.2 cm−1 and 727.5 cm−1 (P–N–C) appeared.17,18,23 With increasing time, these absorbing peaks increased in intensity in the range from 328 to 418 °C. The results indicate that some non-flammable volatiles, such as benzene ring containing, nitrogen-containing, carbon–hydrogen-containing and phosphorus-containing products are generated during the thermal degradation of DPPIP.
image file: c7ra09868e-f8.tif
Fig. 8 FTIR spectra of the gaseous products of DPPIP during the thermal degradation under N2 atmosphere.

To further demonstrate the flame retardant mechanism of DPPIP, the prolyzed products of DPPIP were characterized with py-GC/MS measurement and the results are shown in Fig. 9, Table 6 and Scheme 2. It was found that the pyrolysis behavior of DPPIP is very complicated. When DPPIP is heated up to 600 °C, a small molecule like CO2 is produced at first. With increasing time, more than twenty-three kinds of pyrolysis product were detected, which could be mainly summarized as three kinds of component. The first one was composed of piperazine and its derivatives, including the peaks at 2 (piperazine), 4 (pyrazine), 6 (3-ethylpyrrole), 7 (2-methylpyrazine), 8 ((E)-but-2-ene), 11 (2-methylimidazole) and 16 (4,4′-bipyridine), which were obtained from direct breaks of the piperazine ring and its rearrangement into decomposition segments.23,24 The second one consisted of the compounds with aromatic structures (peaks at 3, 5, 9, 13, 14 and 15), including the benzene ring and its derivatives. These aromatic derivatives occurred following the rupture of P–Ar. And last, lots of phosphorus-containing structures were detected, corresponding to the peaks at 10, 12, 17, 18, 19, 20, 21, 22 and 23.24–26 The phosphorus-containing structures could produce PO free radicals to capture active free radicals such as H and hydrocarbon free radicals during combustion.26 Generally, the result of Py-GC/MS is consistent with those of the TG-FTIR and CC tests.


image file: c7ra09868e-f9.tif
Fig. 9 Pyrograms of DPPIP.
Table 6 Compounds identified from the pyrograms of DPPIP
Peak Retention time (min) m/z Compounds Assigned structure
1 1.70 44 Carbon dioxide O[double bond, length as m-dash]C[double bond, length as m-dash]O
2 2.39 86 Piperazine image file: c7ra09868e-u1.tif
3 2.85 78 Benzene image file: c7ra09868e-u2.tif
4 3.99 80 Pyrazine image file: c7ra09868e-u3.tif
5 4.47 92 Toluene image file: c7ra09868e-u4.tif
6 5.38 95 3-Ethylpyrrole image file: c7ra09868e-u5.tif
7 5.60 94 2-Methylpyrazine image file: c7ra09868e-u6.tif
8 6.37 56 (E)-But-2-ene image file: c7ra09868e-u7.tif
9 6.94 104 Ethenylbenzene image file: c7ra09868e-u8.tif
10 7.46 110 Phenylphosphineinhexane image file: c7ra09868e-u9.tif
11 7.64 82 2-Methylimidazole image file: c7ra09868e-u10.tif
12 8.03 124 White phosphorus P4
13 9.35 107 Methylphenylamine image file: c7ra09868e-u11.tif
14 14.84 154 Biphenyl image file: c7ra09868e-u12.tif
15 15.58 168 2-Methylbiphenyl/4-methylbiphenyl image file: c7ra09868e-u13.tif
16 15.78 156 4,4′-Bipyridine image file: c7ra09868e-u14.tif
17 17.60 186 Diphenylphosphin image file: c7ra09868e-u15.tif
18 18.07 200 Methyldiphenylphosphine image file: c7ra09868e-u16.tif
19 18.84 214 Ethyldiphenylphosphine image file: c7ra09868e-u17.tif
20 20.66 201 Diphenylphosphinoamine image file: c7ra09868e-u18.tif
21 23.25 262 Triphenylphosphine image file: c7ra09868e-u19.tif
22 24.25 242 Diphenylpropenyl phosphine oxide image file: c7ra09868e-u20.tif
23 25.54 260 Ethylenediamine phosphine oxide image file: c7ra09868e-u21.tif



image file: c7ra09868e-s2.tif
Scheme 2 Speculative pyrolysis products of DPPIP at 600 °C.

Based on the Py-GC/MS and FTIR-TG results, the effect of the gaseous phase on the flame retardation of PP is concluded as follows. With increasing temperature, lots of piperazine and its derivatives deriving from direct breaks of the piperazine ring and its rearrangement into decomposition segments are formed and released firstly; meanwhile, the P–Ar bonds break and aromatic structures are produced, which can further increase the amount of inflammable volatile gas. Besides, the rest of the P–Ar bonds continue to be degraded and rearranged, and some structures containing P are finally generated, which can capture active free radicals during the burning.26 Furthermore, the three kinds of inflammable volatile gases can reduce the oxygen content and capture active free radicals during combustion through the gaseous flame retardance mode, resulting in a superior flame-retardant efficiency of PP.

4. Conclusion

A mono-component flame retardant named DPPIP was prepared in this work. PP/DPPIP showed excellent thermal stability and water resistance: the thermal decomposition temperature of the PP/25 wt% DPPIP composite at 5 wt% weight loss is 287.5 °C under air atmosphere, and the weight loss was only about 0.52 wt% after the water treatment. Meanwhile, PP/DPPIP exhibited excellent flame-retardant efficiency. The LOI value of PP/DPPIP reached 27.0%, and passed the V-0 rating at 25 wt% DPPIP. The CC data showed that the PHRR and low THR etc., especially the FGR, largely decreased compared with the corresponding values of neat PP. Furthermore, there was almost no char residue left. The study on the flame retardant mechanism of DPPIP indicated that lots of inflammable gaseous phase products are produced, such as piperazine and its derivatives, and phosphorus-containing structures, which finally lead to a better flame retardant performance for PP.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was financially supported by the National Natural Science Foundation of China (grant number 51703011; 21504015; 51603018); Project of Jilin Provincial Department of Education (grant no. 2016329); Program of Jilin Provincial Department of Science & Technology (grant no. 20170520125JH); and Natural Science Foundation of Fujian Province of China (grant number 2015J05094).

References

  1. K. C. Mai, Z. J. Li, Y. X. Qiu and H. M. Zeng, J. Appl. Polym. Sci., 2001, 80, 2617–2623 CrossRef CAS.
  2. J. Z. Liang, J. Q. Feng, C. P. Tsui, D. F. Liu, S. D. Zhang and W. F. Huang, Composites, Part B, 2015, 71, 74–81 CrossRef CAS.
  3. X. L. Chen, J. Yu, M. He, S. Y. Guo, Z. Luo and S. J. Lu, J. Polym. Res., 2009, 16, 357–362 CrossRef CAS.
  4. Q. H. Tang, R. J. Yang, Y. Song and J. Y. He, Ind. Eng. Chem. Res., 2014, 53, 9728–9737 CrossRef CAS.
  5. Y. Liu, C. L. Deng, J. Zhao, J. S. Wang, L. Chen and Y. Z. Wang, Polym. Degrad. Stab., 2011, 96, 363–370 CrossRef CAS.
  6. X. J. Lai, S. Tang, H. Q. Li and X. R. Zeng, Polym. Degrad. Stab., 2015, 113, 22–31 CrossRef CAS.
  7. H. L. Xie, X. J. Lai, R. M. Zhou, H. Q. Li, Y. J. Zhang, X. R. Zeng and J. H. Guo, Polym. Degrad. Stab., 2015, 118, 167–177 CrossRef CAS.
  8. G. Camino, N. Grassie and I. McNeill, J. Polym. Sci., Polym. Chem. Ed., 1978, 16, 95–106 CrossRef CAS.
  9. Y. L. Wang, X. M. Zhang, A. Li and M. Li, Chem. Commun., 2015, 51, 14801–14804 RSC.
  10. M. C. Yewa, N. H. Ramli Sulong, M. K. Yew, M. A. Amalina and M. R. Johan, Prog. Org. Coat., 2015, 81, 116–124 CrossRef.
  11. C. Y. Luo, J. D. Zuo, F. Q. Wang, Y. C. Yuan, F. Lin, H. H. Huang and J. Q. Zhao, Polym. Degrad. Stab., 2016, 129, 7–11 CrossRef CAS.
  12. Z. Z. Xu, J. Q. Huang, M. J. Chen, Y. Tan and Y. Z. Wang, Polym. Degrad. Stab., 2013, 98, 2011–2020 CrossRef CAS.
  13. K. Yang, M. J. Xu and B. Li, Polym. Degrad. Stab., 2013, 98, 1397–1406 CrossRef CAS.
  14. P. Y. Wen, X. M. Feng, Y. C. Kan, Y. Hu and R. K. K. Yuen, Polym. Degrad. Stab., 2016, 134, 202–210 CrossRef CAS.
  15. Z. J. Wang, Y. F. Liu and J. Li, ACS Sustainable Chem. Eng., 2017, 5, 2375–2383 CrossRef CAS.
  16. Z. B. Shao, C. Deng, Y. Tan, M. J. Chen, L. Chen and Y. Z. Wang, Polym. Degrad. Stab., 2014, 106, 88–96 CrossRef CAS.
  17. Z. B. Shao, C. Deng, Y. Tan, M. J. Chen, L. Chen and Y. Z. Wang, ACS Appl. Mater. Interfaces, 2014, 6, 7363–7370 CAS.
  18. Z. B. Shao, C. Deng, Y. Tan, L. Yu, M. J. Chen, L. Chen and Y. Z. Wang, J. Mater. Chem. A, 2014, 2, 13955–13965 CAS.
  19. H. J. Lin, H. Yan, B. Liu, L. Q. Wei and B. S. Xu, Polym. Degrad. Stab., 2011, 96, 1382–1388 CrossRef CAS.
  20. C. L. Deng, C. Deng, J. Zhao, R. M. Li, W. H. Fang and Y. Z. Wang, Chin. J. Polym. Sci., 2015, 33, 203–214 CrossRef CAS.
  21. H. Breulet and T. Steenhuizen, Polym. Degrad. Stab., 2005, 88, 150–158 CrossRef CAS.
  22. Y. W. Yan, L. Chen, R. K. Jian, S. Kong and Y. Z. Wang, Polym. Degrad. Stab., 2012, 97, 1423–1431 CrossRef CAS.
  23. Thermal and fire performance of flameretarded epoxy resin: investigating interaction between resorcinol bis(diphenyl phosphate) and epoxin nanocomposites, ed. C. Katsoulis, E. Kandare, B. K. Kandola, T. R. Hull and B. K. Kandola, Royal Society of Chemistry, Cambridge, 2009, vol. 17, pp. 184–205 Search PubMed.
  24. L. P. Dong, C. Deng, R. M. Li, Z. J. Cao, L. Lin, L. Chen and Y. Z. Wang, RSC Adv., 2016, 6, 30436–30444 RSC.
  25. L. P. Dong, C. Deng and Y. Z Wang, Polym. Degrad. Stab., 2017, 135, 130–139 CrossRef CAS.
  26. R. K. Jian, P. Wang, W. S. Duan, J. S. Wang, X. L. Zheng and J. B. Weng, Ind. Eng. Chem. Res., 2016, 55, 11520–11527 CrossRef CAS.

This journal is © The Royal Society of Chemistry 2017