Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Characterization of biodegradable poly(lactic acid) porous scaffolds prepared using selective enzymatic degradation for tissue engineering

Ziqi Guoabc, Cheng Yangbc, Zuping Zhoubc, Shan Chen*a and Fan Li*a
aSchool of Life Sciences, Northeast Normal University, Changchun, 130024, China. E-mail: chens093@nenu.edu.cn; lif885@nenu.edu.cn
bSchool of Life Sciences, Guangxi Normal University, Guilin, 541004, China
cGuangxi Universities Key Laboratory of Stem Cell and Biopharmaceutical Technology, Guangxi Normal University, Guilin 541004, China

Received 28th March 2017 , Accepted 5th June 2017

First published on 6th July 2017


Abstract

In this study, poly(lactic acid) (PLA) scaffolds were prepared by selective enzymatic degradation using poly(3-hydrobutyrate-co-4-hydrobutyrate) [P(3HB-co-4HB)] depolymerase. The porous morphology and properties of the scaffolds were investigated to clarify whether the microstructure of the biomimetic extracellular matrix is suitable for cell proliferation and differentiation. When the P(3HB-co-4HB) composition of PLA/P(3HB-co-4HB) blends was changed from 50 wt% to 60 wt%, the mean pore diameter of the porous PLA scaffolds increased from 64.15 µm to 80.01 µm, the porosity significantly improved from 68.45% to 79.88%, and the compressive modulus decreased from 9.34 MPa to 6.94 MPa. PLA40 with 60% P(3HB-co-4HB) blending was used in in vitro degradation and mouse embryo fibroblast (MEF) cell culture tests. The results demonstrated that the PLA scaffolds were degraded completely into harmless products in simulated body fluid (SBF) solution at a slow degradation rate, and the weight loss of the scaffolds could reach 80% after 8 months of in vitro degradation. Meanwhile, the PLA scaffolds showed the largest swelling value of 157.4% after immersion in SBF solution for 14 days. Cell viability was determined through scanning electron microscopy (SEM) and 3-(4,5-dimethyl-2-thiazolyl)-2,5-diphenyl-2-H-tetrazolium bromide (MTT) tests. The results showed that the PLA scaffolds supported the attachment and growth of MEF cells. Compared with the PLA scaffolds without any modification, the PLA scaffolds modified by poly-L-lysine exhibited a better biocompatibility to MEF cells. These results indicate that selective enzymatic degradation has a potential application in scaffold manufacturing.


1. Introduction

Tissue engineering (TE) is a multidisciplinary effort to reconstruct functional tissues and organs following trauma, end stage organ failure, and congenital abnormalities.1,2 In addition, the limitation of organ and tissue transplantations has driven the development of TE3–6, in which new tissues are created from cultured cells and biomaterials. TE, which involves polymer scaffolds, tissue cells, and stimulation factors, has been widely used as an attractive therapeutic treatment for tissue defects.7,8

The major challenges in TE are the preparation of porous scaffolds that can mimic special structures for cell attachment and growth.9,10 In general, TE scaffolds possess a complex interconnected porous micro-hole structure that could enhance various cellular functions, such as adhesion, migration, proliferation, differentiation, and tissue morphologies.11–15 Porous scaffolds should feature not only suitable mechanical properties to support tissues at implantation sites but also biocompatible and biodegradable properties with controllable degradation rates.16–18 Scaffolds serve as a replacement to the natural extracellular matrix (ECM) until host cells could repopulate and synthesize a new natural matrix.

In recent years, many biodegradable materials have been used to fabricate TE scaffolds; these materials include poly(lactic acid) (PLA), poly(ε-caprolactone) (PCL), poly(lactide-co-glycolide), poly(vinyl alcohol), poly(butylene succinate) (PBS), poly(3-hydrobutyrate) (PHB), and poly(3-hydrobutyrate-co-4-hydrobutyrate) [P(3HB-co-4HB)]19–25. Given its absorbability and non-toxicity, PLA has been approved by the US Food and Drug Administration as a biodegradable and biocompatible polymer for use in human body. PLA scaffolds have been prepared by various methods, such as selective vacuum manufacturing, high-pressure molding, salt leaching, and supercritical fluid technology.26–31 Many conventional techniques, including phase separation and particulate leaching, have been used and improved to fabricate PLA scaffolds by removing one or two phases from the multiphase blend.32–35 However, these techniques usually demonstrate restricted capabilities to control pore characteristics, avoid toxic chemical reagents, and generate an internal pore network within the scaffolds. Selective enzymatic degradation, in which one phase is removed from blends, is an alternative technique to prepare porous scaffolds.36–38 Liu39 reported that PLA scaffolds could be prepared through the selective enzymatic degradation of PCL. However, whether scaffolds prepared by selective enzymatic degradation could be used in TE has yet to be determined. Although various preparation methods have been developed and improved to fabricate an ideal TE scaffold, a clinically useful tissue scaffold remains undeveloped to date.

In the present study, we fabricated an ideal porous scaffold by selective enzymatic degradation. Depolymerase with the substrate specificity of P(3HB-co-4HB) was adopted to degrade and remove P(3HB-co-4HB) from PLA/P(3HB-co-4HB) blends, and various porous PLA scaffolds were acquired by changing the ratio of PLA/P(3HB-co-4HB) blend films. The properties and biocompatibility of the scaffolds were evaluated in detail. Results show that selective enzymatic degradation is a promising method to prepare porous scaffolds for TE.

2. Experimental

2.1 Materials

PLA commercially available from Nature works LLC (USA) was used in this work. It exhibited a weight-average molecular weight of 2.07 × 105 g mol−1 and a polydispersity of 1.74 as determined by gel permeation chromatography (GPC). P(3HB-co-4HB) was provided by Tianjin Guoyun Biotech (Tianjin, China). It exhibited a weight-average molecular weight of 4.97 × 105 g mol−1 and a polydispersity of 1.85 (GPC). The 4HB content in the copolymer was 6.5 mol% as determined by 1H-nuclear magnetic resonance spectroscopy. P(3HB-co-4HB) depolymerase is a novel poly(hydroxybutyrate)-degradable esterase purified from Agrobacterium sp. DSGZ isolated in our laboratory.40

2.2 Blend preparation

Before processing, PLA and P(3HB-co-4HB) were dried at 80 °C in a vacuum oven for 24 h. PLA/P(3HB-co-4HB) blends at different weight ratios (wt/wt: 10/90, 20/80, 30/70, 40/60, 50/50, 60/40, 70/30, 80/20, 90/10) were prepared using a Haake batch internal mixer (Haake Rheomix600, Karlsruhe, Germany) with a batch volume of 50 mL. Melt compounding was performed at 175 °C and a screw speed of 50 rpm for 8 min until the viscosity had reached a nearly constant value. After mixing, all samples were cut into small pieces, hot-pressed at 180 °C for 3 min, and then cold-pressed at room temperature to form sheets with a thickness of 0.6 cm or 0.2 cm. The compression molding steps were carried out carefully to impose the same treatment to each sample.

2.3 Selective enzymatic degradation

Selective enzymatic degradation was conducted to remove the P(3HB-co-4HB) component from the blends and obtain the corresponding porous PLA scaffolds. The enzymatic degradation of the blends for P(3HB-co-4HB) was carried out in phosphate buffer (pH 7.5) containing P(3HB-co-4HB) depolymerase (0.2 mg mL−1) at 50 °C with shaking at 100 rpm, and the enzymatic solution was replaced each 12 h. When the P(3HB-co-4HB) component in the sample was degraded completely, the sample was removed, washed with distilled water, and then dried to constant weight in a vacuum.

2.4 Morphology analysis

The appearance of the blends before and after selective enzymatic degradation was obtained using a digital camera, and the microstructure of the PLA scaffolds was observed by scanning electron microscopy (SEM, XL30 ESEM FEG, FEI Co., Eindhoven, The Netherlands). The blends were stored in liquid nitrogen and then brittle fractured. Cryo-fractured surfaces of PLA/P(3HB-co-4HB) blends were observed via SEM to examine the phase structure. Based on the SEM images, the pore diameter and standard deviation were analyzed with an image analysis program (Adobe Photoshop 7.0). 50 random pores on the surface of PLA scaffolds were chosen in each groups to calculate and normalize the pore size.41

2.5 Porosity

The porosity of the three rectangular cube specimens was determined using Archimedes' principle, and ethanol was used as liquid medium.42,43 The porosity was calculated via the following equation:
Porosity (%) = (m2m1)/(m2m3) × 100,
where m1 is the dry weight of PLA scaffolds, m2 is the weight of PLA scaffolds immersed in ethanol, and m3 is the weight of PLA scaffolds suspended in ethanol. Three samples were tested to calculate the average porosity.

2.6 Mechanical properties

The mechanical properties of the PLA scaffolds (1.0 cm × 1.0 cm × 0.6 cm) were tested in accordance with ISO: 604-02 by using a universal testing machine (Instron-1121, USA) at room temperature. A crossed speed of 0.2 mm min−1 and a 5000 N load range were used in the mechanical tests. Values were averaged, and the standard deviation of at least three specimens was calculated.

2.7 In vitro degradation study

PLA scaffolds were cut into films (1.0 cm × 1.0 cm × 0.2 cm) for in vitro degradation study. The films were placed in sealed Petri plates containing simulated body fluid (SBF) and then incubated in vitro at 100 rpm and 37 °C. The SBF solution used was reported by Tadashi Kokubo,44 and it contained NaCl (136.8 mM), NaHCO3 (4.2 mM), KCl (3.0 mM), K2HPO4 (1.0 mM), MgCl2·6H2O (1.5 mM), CaCl2 (2.5 mM), and NaSO4 (0.5 mM). The pH of the buffer was adjusted to 7.5 with (CH2OH)3CNH2 and HCl. The SBF solution was replaced every 3 days to avoid any pH changes that may affect the degradation of the sample. After a predetermined time of in vitro degradation, each blend film was washed with distilled water and then dried in vacuum. Finally, the weight loss of each sample was measured.

2.8 Water absorption of the PLA scaffolds

To ensure that the SBF solution could permeate the porous PLA scaffolds thoroughly, the scaffolds were pre-wetted by SBF solution and then immersed in 50 mL of SBF solution at 37 °C for different periods (7, 14, 21, and 28 days). After immersion, the scaffolds were carefully wiped with filter paper to remove the surface water, and then the weights of the scaffolds were measured as Wwet. The dry weights of the scaffolds were measured as Wdry before the absorption test.

The water adsorption capacity of the PLA scaffolds was characterized in terms of the swelling percentage (Sw), which was calculated using the following equation:45

Sw = (WwetWdry)/Wdry × 100.

At least three specimens were tested for each sample to obtain an average value.

2.9 Cell attachment on the PLA scaffolds

Mouse embryo fibroblast cells purchased from Sigma of Life Science were cultured in Dulbecco's modified Eagle's medium (DMEM, GIBACO, USA) containing 10% fetal bovine serum (FBS, Hyclone, China) and 1% antibiotic/antimycotic solution (100 U mL−1 penicillin and 100 µg mL−1 streptomycin, Sigma) at 37 °C with 5% humidified CO2. MEF cells were seeded with a density of 1 × 105 cells/sample in a six-well plate containing the PLA scaffolds. Before culturing cells, the PLA scaffolds were sterilized with 75% ethanol for 1 h, washed with PBS for three times, and then exposed to UV light for 2 h. Sterile PLA scaffolds were immersed in DMEM at 37 °C with 5% humidified CO2 for 24 h, and MEF cells (1 × 105 cells per sample) were evenly dropped onto the top of the scaffolds. The cell-seeded PLA scaffolds were cultured at 37 °C with 5% humidified CO2 for 1, 3, and 7 days, and the medium was replaced every 2 days. The cell-scaffold constructs were fixed in 2.5% glutaraldehyde for 2 h, dehydrated with a graded series of ethanol solutions (50%, 70%, 80%, 90%, and absolute ethanol), dried in vacuum, sputter-coated with gold, and then viewed using SEM.46

2.10 Cell viability

A 3-(4,5-dimethyl-2-thiazolyl)-2,5-diphenyl-2-H-tetrazolium bromide (MTT) test was performed to detect cell viability, which is an indicator to evaluate the cell biocompatibility or cytotoxicity of the PLA scaffolds. The MTT test is a colorimetric assay in which the amount of the pale yellow MTT formazan complex is measured and is directly proportional to the number of living cells. PLA scaffolds were immersed in DMEM containing 10% FBS and 1% antibiotic/antimycotic solution at 37 °C for 12 h, and the conditional DMEM was used to culture MEF cells in 96-well plates. A tissue culture plate adding fresh DMEM without PLA scaffolds was used as a positive control. MEF cells at 5 × 104 cells per mL were seeded on a 96-well plate containing 200 µL of DMEM medium. During culture, the medium in each well was replaced every 2 days by the relative medium (200 µL). After culturing for 1, 4, and 7 days, 20 µL of MTT solution (20 mM) was added into each well, and then cells were cultured at 37 °C with 5% humidified CO2 for 4 h to allow MTT reduction by mitochondrial dehydrogenase in viable cells. The DMEM medium was replaced with 200 µL of dimethyl sulfoxide to solubilize the formazan complex, and then the 96-well plates were slightly vibrated to ensure that the formazan completely dissolved. The UV absorbance of the solution in each well at 490 nm was measured using a microplate reader.47 All MTT tests were performed with three replicates.

2.11 Surface modification of PLA scaffolds

Porous PLA scaffolds were prepared by selective enzymatic degradation. PLA60 scaffolds were placed in poly-L-lysine (PLL) solution (1.0 g L−1) and then negative pressure exhaust was performed to modify the surfaces of the PLA scaffolds.48 The modified PLA scaffolds were autoclaved, and their biocompatibility to MEF cells was investigated. MEF cells were cultured both on PLA60 scaffolds and modified PLA60 scaffolds. After 1, 4, and 7 days of culture, cell viability was evaluated by MTT test as described above.

2.12 Statistical analysis

Quantitative data were presented as mean ± standard deviation. The statistical analysis for significance between the groups was performed by means of Student's t-test using SPSS13.0 software. A confidence level of 95% (p < 0.05) was considered to be statistically significant. Each cell culture experiment was performed in triplicate.

3. Results and discussion

3.1 Preparation of PLA scaffolds

3.1.1 Phase separation of PLA/P(3HB-co-4HB) blends. The morphologies of blends are strongly influenced by the properties of the polymer in the blends. Thomas et al.49,50 have studied the blending of PLA/PHB and PLA/poly (3-hydroxybutyrate-co-3-hydroxyvalerate) prepared by melt compounding, and found that the blends are immiscible in any type of compositions. In the present study, dynamic mechanical analysis showed that PLA/P(3HB-co-4HB) was an immiscible system with the P(3HB-co-4HB) domains evenly dispersed in the PLA matrix (data not shown). This result provided a possibility to prepare porous biodegradable polyester materials by the removal of one component from the binary phase-separated biodegradable polyester blends using selective enzymatic hydrolysis and subsequent elution of the formed water-soluble oligomers and monomers into the surrounding hydrolysis media.

The phase structures of the PLA/P(3HB-co-4HB) blends were observed by SEM, and the fracture surface micrographs of the blends with P(3HB-co-4HB) compositions are shown in Fig. 1(a and b). The PLA/P(3HB-co-4HB) blends showed co-continuous morphology, and both the blends were immiscible when the P(3HB-co-4HB) composition of the blends was changed from 50 wt% to 60 wt%.


image file: c7ra03574h-f1.tif
Fig. 1 The change of PLA/P(3HB-co-4HB) blends via enzymatic degradation: (a) SEM micrographs of the fractured surfaces of blends with the weight ratio (wt/wt, 50/50) after selective enzymatic degradation; (b) SEM micrographs of the fractured surfaces of blends with the weight ratio (wt/wt, 40/60) after selective enzymatic degradation; (c) weight loss curve of the blends; (d) external morphology of PLA/P(3HB-co-4HB) blends without degradation; (e) external morphology of PLA/P(3HB-co-4HB) blends after degradation.
3.1.2 Selective enzymatic degradation. A series of PLA/P(3HB-co-4HB) blends with a variety of compositions (wt/wt: 10/90, 20/80, 30/70, 40/60, 50/50, 60/40, 70/30, 80/20, 90/10) have been used to prepare porous PLA scaffolds, however, only 50/50 and 60/40 recipes could build stable porous structure and high porosity. Therefore, PLA/P(3HB-co-4HB) blends with the weight ratios (50/50 and 40/60, wt/wt) were prepared by melt blending and hot pressing. P(3HB-co-4HB) depolymerase purified from Agrobacterium sp. DSGZ was used to degrade P(3HB-co-4HB) in PLA/P(3HB-co-4HB) blends because of its substrate specificity for degrading polyhydroxyalkanoates but not PLA.40 As shown in Fig. 1c, the weight loss of the PLA/P(3HB-co-4HB) blends increased with degradation time. The weight loss of the PLA/P(3HB-co-4HB) blends (50/50, wt/wt) reached 49.82% after 27 days of enzymatic degradation. The weight loss of the PLA/P(3HB-co-4HB) blend films (40/60, wt/wt) increased to 59.88% after 21 days of enzymatic degradation. The weight loss remained constant with further degradation, suggesting that the P(3HB-co-4HB) component in the blends was completely degraded, and the remaining might be PLA component.

Before enzymatic degradation, the surface of the PLA/P(3HB-co-4HB) blends was smooth, and its color was pale yellow. However, the surface of the blends became rougher, and its color turned white after degradation (Fig. 1d and e). With the selective degradation of P(3HB-co-4HB), the composition of the scaffolds was mainly PLA, and the color of the scaffolds was white. P(3HB-co-4HB) on the surface of the blends was degraded preferentially and then turned gradually to internal until it was completely degraded, which consequently caused its surface to become rough. The rough surface morphology of the PLA scaffolds increased the specific surface area and provided suitable surface properties for cell attachment, proliferation, and migration. According to the composition of PLA in the PLA/P(3HB-co-4HB) blends, the remaining PLA scaffolds were named as PLA40 and PLA50, and the number represented the proportion of PLA in the blends.

3.2 Morphology of PLA scaffolds

As illustrated in Fig. 2 and 3, the surface morphologies of the PLA scaffolds prepared by selective enzymatic degradation were observed by SEM. The SEM micrographs of the blends after 15 days of degradation and the remaining PLA scaffolds showed that various pores were distributed evenly onto the surface of the PLA scaffolds. However, the morphology and distribution of the pores significantly differed with the change of the composition of P(3HB-co-4HB) in the blends. Through these results we could conclude that polymer composition and degradation time would significantly influence the porous characterizations of the PLA scaffolds via selective enzymatic degradation.
image file: c7ra03574h-f2.tif
Fig. 2 SEM images of PLA/P(3HB-co-4HB) blends (wt/wt, 50/50) after different degradation times: 15 days of degradation (a, b), 30 days of degradation (c, d).

image file: c7ra03574h-f3.tif
Fig. 3 SEM images of PLA/P(3HB-co-4HB) blends (wt/wt, 40/60) after different degradation times: 15 days of degradation (a, b), 30 days of degradation (c, d).
3.2.1 Effect of polymer composition on porous characterizations. As shown in Fig. 2d and 3d, when the P(3HB-co-4HB) composition in the blends was increased from 50 wt% to 60 wt%, the shape of the pores onto the PLA scaffolds became longer and narrower, and the mean pore diameter increased from 64.15 ± 1.50 to 80.01 ± 1.02 µm (Table 1). In addition, the porosity of the PLA scaffolds was influenced by the P(3HB-co-4HB)/PLA ratio. The porosity in the PLA50 scaffolds was 68.45%, which was lower than the 79.88% porosity in the PLA40 scaffolds. SEM results showed that pores were distributed regularly onto the surface of the PLA scaffolds when the P(3HB-co-4HB) composition was 50 wt% or 60 wt%, and then several pores were distributed within the PLA40 scaffolds and PLA50 scaffolds.
Table 1 Porous properties of PLA scaffolds prepared by selective enzymatic degradation
Scaffolds Degradation period (day) Mean size (µm) Porosity (%) Minimum pore size (µm) Maximum pore size (µm)
PLA50 30 64.15 ± 1.50 68.45 ± 0.88 29.49 104.79
PLA40 15 67.27 ± 1.22 68.55 ± 1.71 31.38 121.07
30 80.01 ± 1.02 79.88 ± 2.02 44.53 113.97


Porous TE scaffolds to be used as replacements of injured living tissues must possess optimal pore microstructure and mechanical properties. TE scaffolds with a mean pore size of 20 µm are conducive to fibroblast growth; scaffolds with a mean pore size of 20–125 µm are suitable for skin regeneration;51,52 Meanwhile, scaffolds with a mean pore size of 100–250 µm favor the regeneration of bone cells.53 In the present study, the pore properties (diameter: 80.01 µm, porosity: 79.88%), good connectivity of the pore microstructure, and uniform pore distribution on the surface of the PLA scaffolds indicated the suitability of the PLA40 scaffolds' porous properties for soft TE applications.

3.2.2 Effect of degradation time on porous characterizations. P(3HB-co-4HB), a biosynthesis and biodegradable polymer with suitable and biocompatibility, is also an alternative for TE scaffolds. The biodegradation products of 3-hydrobutyrate and 4-hydrobutyrate may be common metabolites in higher organisms.54 Therefore, before complete degradation, P(3HB-co-4HB) residue in PLA scaffolds exerts no influence on the biocompatibility of the scaffolds. The effect of degradation time on porous characterizations was investigated. SEM images of the PLA scaffold surface prepared by selective enzymatic degradation for different periods (15 and 30 days) are shown in Fig. 2 and 3. The pore sizes and mean pore diameters were analyzed and are listed in Table 1. Results showed that degradation time significantly influenced the pore sizes and porosities of the scaffolds. After 15 days of degradation, the mean pore size and porosity of the PLA40 scaffolds were 67.27 µm and 68.55%, respectively. When selective enzymatic degradation was prolonged to 30 days, the mean pore size and porosity of the PLA60 scaffolds increased to 80.01 µm and 79.88%, respectively. This result demonstrated that prolonging the degradation time could effectively improve the porous microstructure and characterizations of PLA scaffolds. To the best of our knowledge, this study is the first to optimize the morphological parameters of scaffolds prepared by selective enzymatic degradation. The results suggest that selective enzymatic degradation is suitable to prepare multiple porous scaffolds with different porous structures and porosities by controlling the ratio of blending material composition or the time.

In this study, the PLA40 scaffolds prepared through 30 days of degradation by P(3HB-co-4HB) depolymerase had high porosity, uniform pore distribution, and good connectivity. Such properties widen the application range of scaffolds in TE.55 Therefore, PLA40 scaffolds after absolute degradation were selected in the following experiments.

3.3 Mechanical properties of PLA scaffolds

Mechanical tests were successfully conducted, and the obtained compressive load and elastic modulus of the PLA scaffolds were used to confirm the mechanical properties for the three specimens. The compressive elastic modulus and load of the PLA50 scaffolds were 9.34 ± 0.23 MPa and 523.33 ± 5.81 N, respectively, which were larger than those of the PLA40 scaffolds (6.94 ± 0.54 MPa and 398.33 ± 3.92 N, respectively) as listed in Table 2. TE scaffolds should have the mechanical strength needed to create a macroporous scaffold that could retain its structure after implantation, particularly in the reconstruction of human tissues.56 To achieve a functionally satisfactory implant for practical applications, mechanical properties should be considered in the design of porous scaffolds. Porous scaffolds are suitable for tissue regeneration and organ repair if the compressive modulus of elasticity is between 0.4 MPa and 350 MPa.57,58 In this study, the strength and modulus of the PLA scaffolds conform to the basic mechanical property requirements in TE.
Table 2 Mechanical properties of PLA scaffolds
Scaffolds Compressive load (MPa) Elastic modulus (N)
PLA40 6.94 ± 0.54 398.33 ± 3.92
PLA50 9.34 ± 0.23 523.33 ± 5.81


3.4 Swelling behavior of PLA scaffolds

Swelling behavior is another important index when assessing the application potential of scaffolds in TE because excessive water absorption destroys the morphology of the scaffold while insufficient absorption inhibits cell growth because of the lack of water.59 Gao60 reported the standard of water absorption performance and proposed that scaffolds with water swelling values ranging from 120% to 200% are qualified for TE. In the present study, water absorption was measured to assess the swelling ability of the PLA40 scaffolds. The swelling behavior of the PLA scaffolds in SBF solution is shown in Fig. 4a. After 14 days of immersion in SBF solution, the scaffolds exhibited the largest swelling value (157.4%) and then became swollen. When the immersion time was prolonged, the swelling value did not change. The results demonstrated that the water absorption of the PLA scaffolds met the standard of TE scaffolds.
image file: c7ra03574h-f4.tif
Fig. 4 Swelling behavior (a) and in vitro degradation behavior (b) of PLA scaffolds in SBF solution (pH 7.5) at different incubation time intervals.

3.5 In vitro degradation of PLA scaffolds

The in vitro degradation behavior of the PLA scaffolds after immersion in SBF solution at 37 °C for 240 days is shown in Fig. 4b. The weight loss of the PLA scaffolds increased with incubation time until the 240th day. After immersion in SBF solution for more than 7 days, more weight loss occurred, and the PLA scaffold (about 150 mg) was degraded absolutely after 8 months of incubation. Undoubtedly, TE scaffolds should be completely degraded into nontoxic products to cells, but the degradation rate should be slow to allow the scaffolds to maintain their mechanical structure conducive for cell growth. Pushpa and Shi61 reported that PLA can be hydrolyzed to carbon dioxide and water under certain conditions. In the present study, the PLA scaffolds could also be hydrolyzed into non-toxic products in vitro, and the good biocompatibility of the PLA scaffolds was not affected by their hydrolysis.

3.6 Viability of MEF cells on PLA scaffolds

Biocompatibility is an important characteristic of scaffold materials intended for TE applications. To determine whether the porous PLA scaffolds are suitable for TE applications, MEF cells were seeded on the scaffolds, and the results were investigated by SEM and MTT assay (Fig. 5 and 6).
image file: c7ra03574h-f5.tif
Fig. 5 SEM images of MEF cells on PLA40 scaffolds after 7 days of culture. The red squares indicate adhering cells.

image file: c7ra03574h-f6.tif
Fig. 6 Cell viability after 1, 4, and 7 days of culture on PLA40 scaffolds and PLL-modified PLA40 scaffolds by MTT assay. Student's t-tests were performed on cells on PLA40 scaffolds compared with control cells (*p < 0.05, **p < 0.01).

Fig. 5 displays the SEM images of the PLA scaffolds cultured with 7 days of culture. After culturing, some MEF cells attached onto the surface of the PLA scaffolds. In addition, the majority of MEF cells displayed both scattered single cell and small cell clusters, and exhibited round and spherical morphologies indicating a good cell proliferation. The results demonstrated that MEF cells attached more easily on the surface than in the interior of the PLA40 scaffolds. Cell attachments could be inhibited by bio-polymers with extreme hydrophilicity or hydrophobicity. The morphology of the cells cultured on the scaffolds may be influenced by the hydrophilicity of the TE scaffold materials.47 Poisonous reagents were not added in the entire process of preparation, and PLA and P(3HB-co-4HB) are medical materials. P(3HB-co-4HB) depolymerase could be washed off by sterilized water and 70% ethanol from the PLA scaffolds. Therefore, non-toxic PLA scaffolds with good biocompatibility through selective enzymatic degradation exhibited a great potential in TE.

In order to further improve PLA40 scaffolds' biocompatibility on cells (adhesion, proliferation, and differentiation), the scaffolds were modified by PLL solution. To investigate the effect of the biocompatibility of PLA40 scaffolds through the modification with PLL solution, the viability of MEF cells on porous scaffolds was measured by MTT assay. Meanwhile, the hydrophilicity of PLA40 scaffolds was tested by using Contact Angle tester. From the hydrophilicity test, we found that PLA40 scaffolds modified by PLL solution showed a better hydrophilicity than unmodified PLA40 scaffolds. As displayed in Fig. 6, MEF cells cultured on PLA40 scaffolds and PLL-modified PLA40 scaffolds showed great proliferative potential, and the cell population significantly increased after 1–4 days of culture. According to these results, we hypothesized the hydrophilicity of scaffolds could increase its biocompatibility, and the remaining hydrophobicity of PLA40 scaffolds leaded to a slightly low level of viability compared with the control group cells after 7 days of culture. The viability of MEF cells on the PLL-modified PLA40 scaffolds were significantly higher than those on the PLA40 scaffolds after 7 days of culture, and the results indicated that PLA40 scaffolds' hydrophilicity has been strengthened and then its biocompatibility improved consequently. Compared with the control group, MEF cells' proliferation ability onto PLA40 scaffolds modified by PLL solution kept 90% after 7 days of culture, therefore we're sure PLA40 scaffolds showed a good biocompatibility. Similar results have previously been observed by Ramakrishna's group62,63 using poly(L-lactide-co-ε-caprolactone)-based scaffolds. According to Yang et al.,64 an appropriate combination of hydrophobicity/hydrophilicity associated with surface properties remains a substantial factor able to influence cell adhesion and proliferation on biomaterials.

4. Conclusion

Novel biomorphic PLA scaffolds were successfully prepared by selective enzymatic degradation. Characteristic tests suggested that porous PLA scaffolds provided good surface and internal structure for cell adhesion and growth. In addition, the mechanical strength, in vitro degradation, and swelling behavior of the PLA scaffolds met the requirements in TE. The blending material composition and degradation time can influence the porous structure of the scaffolds. This advantage renders selective enzymatic degradation applicable in TE requiring different pore structures.

Acknowledgements

This work was supported by National Natural Science Foundation of China (No. 31670122) and Scientific and Technological Planning Project of Ji Lin (No. 20150520032JH).

Notes and references

  1. M. Ueda, Tanpakushitsu Kakusan Koso, 2000, 45, 2257–2259 CAS.
  2. V. Marx, Nature, 2015, 522, 373–377 CrossRef CAS PubMed.
  3. P. Hernigou, Int. Orthop., 2015, 39, 807–817 CrossRef PubMed.
  4. J. A. Panadero, L. Vikingsson, J. L. Gomez Ribelles, S. Lanceros-Mendez and V. Sencadas, J. Biomed. Mater. Res., Part B, 2015, 103, 1037–1043 CrossRef CAS PubMed.
  5. G. A. Mandelaris, D. B. Spagnoli, A. L. Rosenfeld, J. McKee and M. Lu, Int. J. Periodontics Restorative Dent., 2015, 35, 325–333 Search PubMed.
  6. M. J. Danesh-Meyer, Ann. R. Australas. Coll. Dent. Surg., 2000, 15, 144–149 CAS.
  7. A. K. Lynn, R. A. Brooks, W. Bonfield and N. Rushton, J. Bone Jt. Surg., Br. Vol., 2004, 86, 1093–1099 CrossRef CAS.
  8. M. V. Risbud and M. Sittinger, Trends Biotechnol., 2002, 20, 351–356 CrossRef CAS PubMed.
  9. Y. K. Kurokawa and S. C. George, Adv. Drug Delivery Rev., 2016, 96, 255–233 CrossRef PubMed.
  10. O. D. Baydik, M. A. Titarenko and P. G. Sysolyatin, Stomatologiia, 2015, 94, 65–68 CrossRef CAS PubMed.
  11. A. Panda, Indian J. Urol., 2015, 31, 87–88 CrossRef PubMed.
  12. X. Zhang and Y. Zhang, Cell Biochem. Biophys., 2015, 72, 777–782 CrossRef CAS PubMed.
  13. G. Jin, G. H. Yang and G. Kim, J. Biomed. Mater. Res., Part B, 2015, 103, 935–948 CrossRef PubMed.
  14. S. P. Pilipchuk, A. B. Plonka, A. Monje, A. D. Taut, A. Lanis, B. Kang and W. V. Giannobile, Dent. Mater., 2015, 31, 317–338 CrossRef CAS PubMed.
  15. M. Borjigin, C. Eskridge, R. Niamat, B. Strouse, P. Bialk and E. B. Kmiec, Int. J. Nanomed., 2013, 8, 855–864 Search PubMed.
  16. E. Quinlan, A. Lopez-Noriega, E. Thompson, H. M. Kelly, S. A. Cryan and F. J. O'Brien, J. Controlled Release, 2015, 198, 71–79 CrossRef CAS PubMed.
  17. X. He, L. Cheng, X. Zhang, Q. Xiao, W. Zhang and C. Lu, Carbohydr. Polym., 2015, 115, 485–493 CrossRef CAS PubMed.
  18. J. Pu and K. Komvopoulos, Acta Biomater., 2014, 10, 2718–2726 CrossRef CAS PubMed.
  19. A. Dogan, S. Demirci, Y. Bayir, Z. Halici, E. Karakus, A. Aydin, E. Cadirci, A. Albayrak, E. Demirci, A. Karaman, A. K. Ayan, C. Gundogdu and F. Sahin, Mater. Sci. Eng., C, 2014, 44, 246–253 CrossRef CAS PubMed.
  20. M. Zhou and D. Yu, Mol. Med. Rep., 2014, 10, 508–514 CAS.
  21. A. Przekora, K. Palka and G. Ginalska, J. Biotechnol., 2014, 182–183, 46–53 CrossRef CAS PubMed.
  22. N. Thadavirul, P. Pavasant and P. Supaphol, J. Biomed. Mater. Res., Part A, 2014, 102, 3379–3392 CrossRef PubMed.
  23. W. Fu, Z. Liu, B. Feng, R. Hu, X. He, H. Wang, M. Yin, H. Huang, H. Zhang and W. Wang, Int. J. Nanomed., 2014, 9, 2335–2344 CrossRef PubMed.
  24. C. L. Zhang, K. P. Lv, H. P. Cong and S. H. Yu, Small, 2012, 8, 647–653 CrossRef CAS PubMed.
  25. K. Mohanraj, S. Sethuraman and U. M. Krishnan, J. Biomed. Mater. Res., Part B, 2013, 101, 840–847 CrossRef PubMed.
  26. Y. I. Yoon, K. E. Park, S. J. Lee and W. H. Park, BioMed Res. Int., 2013, 2013, 309048 Search PubMed.
  27. K. Novotna, M. Zajdlova, T. Suchy, D. Hadraba, F. Lopot, M. Zaloudkova, T. E. Douglas, M. Munzarova, M. Juklickova, D. Stranska, D. Kubies, D. Schaubroeck, S. Wille, L. Balcaen, M. Jarosova, H. Kozak, A. Kromka, Z. Svindrych, V. Lisa, K. Balik and L. Bacakova, J. Biomed. Mater. Res., Part A, 2014, 102, 3918–3930 CrossRef PubMed.
  28. A. M. Haaparanta, E. Jarvinen, I. F. Cengiz, V. Ella, H. T. Kokkonen, I. Kiviranta and M. Kellomaki, J. Mater. Sci.: Mater. Med., 2014, 25, 1129–1136 CrossRef CAS PubMed.
  29. C. R. Almeida, T. Serra, M. I. Oliveira, J. A. Planell, M. A. Barbosa and M. Navarro, Acta Biomater., 2014, 10, 613–622 CrossRef CAS PubMed.
  30. L. G. Santos, D. C. Oliveira, M. S. Santos, L. M. Neves, F. O. de Gaspi, F. A. Mendonca, M. A. Esquisatto, G. M. Santos, M. A. d'Avila and L. H. Mei, J. Nanosci. Nanotechnol., 2013, 13, 4694–4702 CrossRef CAS PubMed.
  31. S. Roman, A. Mangera, N. I. Osman, A. J. Bullock, C. R. Chapple and S. MacNeil, Neurourol. Urodyn., 2014, 33, 531–537 CrossRef CAS PubMed.
  32. G. T. Hoffman, E. C. Soller and K. M. McNally-Heintzelman, Biomed. Sci. Instrum., 2002, 38, 53–58 CAS.
  33. N. K. Mekala, R. R. Baadhe, S. R. Parcha and P. D. Yalavarthy, J. Biomed. Res., 2013, 27, 318–325 CAS.
  34. R. Scaffaro, F. Lopresti, L. Botta, S. Rigogliuso and G. Ghersi, J. Mech. Behav. Biomed. Mater., 2015, 54, 8–20 CrossRef PubMed.
  35. X. Zhu, T. Zhong, R. Huang and A. Wan, J. Biomater. Sci., Polym. Ed., 2015, 26, 1286–1296 CrossRef CAS PubMed.
  36. C. H. Wang, K. R. Fan and G. H. Hsiue, Biomaterials, 2005, 26, 2803–2811 CrossRef CAS PubMed.
  37. L. M. Pitet, M. A. Amendt and M. A. Hillmyer, J. Am. Chem. Soc., 2010, 132, 8030–8031 CrossRef PubMed.
  38. L. J. Liu, L. M. Li, G. Henri and V. Michel, Biomacromolecules, 2000, 1, 350–359 CrossRef CAS PubMed.
  39. T. Hideto and I. Takeharu, Macromol. Biosci., 2001, 1, 59–65 CrossRef.
  40. Z. Q. Guo, F. Li, D. Liu, B. H. M. Xia, C. Yang, S. Chen and Y. F. Yang, J. Appl. Polym. Sci., 2015, 133 DOI:10.1002/app.42805.
  41. H. Liu, S. Wang and N. Qi, J. Appl. Polym. Sci., 2012, 125, E468–E476 CrossRef CAS.
  42. N. Johari, M. H. Fathi, M. A. Golozar, E. Erfani and A. Samadikuchaksaraei, J. Mater. Sci.: Mater. Med., 2012, 23, 763–770 CrossRef CAS PubMed.
  43. B. Pick, M. Pelka, R. Belli, R. R. Braga and U. Lohbauer, Dent. Mater., 2011, 27, 664–669 CrossRef CAS PubMed.
  44. T. Kokubo and H. Takadama, Biomaterials, 2006, 27, 2907–2915 CrossRef CAS PubMed.
  45. N. Kathuria, A. Tripathi, K. K. Kar and A. Kumar, Acta Biomater., 2009, 5, 406–418 CrossRef CAS PubMed.
  46. J. Qian, X. Yong, W. Xu and X. Jin, Mater. Sci. Eng., C, 2013, 33, 4587–4593 CrossRef CAS PubMed.
  47. N. M. Alves, J. Shi, E. Oramas, J. L. Santos, H. Tomas and J. F. Mano, J. Biomed. Mater. Res., Part A, 2009, 91, 480–488 CrossRef PubMed.
  48. R. A. Quirk, W. C. Chan, M. C. Davies, S. J. Tendler and K. M. Shakesheff, Biomaterials, 2001, 22, 865–872 CrossRef CAS PubMed.
  49. M. Zhang and N. L. Thomas, Adv. Polym. Technol., 2011, 30, 67–79 CrossRef CAS.
  50. M. R. Nanda, M. Misra and A. K. Mohanty, Macromol. Mater. Eng., 2011, 296, 719–728 CrossRef CAS.
  51. S. S. Kroll, S. Sharma, C. Koutz, H. N. Langstein, G. R. D. Evans, G. L. Robb, D. W. Chang and G. P. Reece, Plast. Reconstr. Surg., 2001, 107, 338–341 CrossRef CAS PubMed.
  52. S. Sercu, M. Zhang, N. Oyama, U. Hansen, A. E. Ghalbzouri, G. Jun, K. Geentjens, L. Zhang and J. H. Merregaert, J. Invest. Dermatol., 2008, 128, 1397–1408 CrossRef CAS PubMed.
  53. B. D. Boyan, T. W. Hummert, D. D. Dean and Z. Schwartz, Biomaterials, 1996, 17, 137–146 CrossRef CAS PubMed.
  54. X. T. Li, Y. Zhang and G. Q. Chen, Biomaterials, 2008, 29, 3720–3728 CrossRef CAS PubMed.
  55. M. M. Rahman, S. Pervez, B. Nesa and M. A. Khan, Polym. Int., 2013, 62, 79–86 CrossRef CAS.
  56. W. L. Grayson, T. P. Martens, G. M. Eng, M. Radisic and G. Vunjak-Novakovic, Semin. Cell Dev. Biol., 2009, 20, 665–673 CrossRef CAS PubMed.
  57. X. H. Wang, S. Shi, G. Guo, S. Z. Fu, M. Fan, F. Luo, X. Zhao, Y. Q. Wei and Z. Y. Qian, J. Biomater. Sci., Polym. Ed., 2011, 22, 1917–1929 CrossRef CAS PubMed.
  58. C. Zhang, Y. Hu, Z. Xiong, S. Zhang, Y. Yan and F. Cui, Zhongguo Xiufu Chongjian Waike Zazhi, 2005, 19, 100–104 CAS.
  59. J. Zhang, H.-M. Yin, B. S. Hsiao, G.-J. Zhong and Z.-M. Li, J. Mater. Sci., 2013, 49, 1648–1658 CrossRef.
  60. C. Gao, X. Hu, Y. Hong, J. Guan and J. Shen, J. Biomater. Sci., Polym. Ed., 2003, 14, 937–950 CrossRef CAS PubMed.
  61. P. G. Shao and L. C. Bailey, Pharm. Dev. Technol., 1999, 4, 633–642 CrossRef CAS PubMed.
  62. M. P. Prabhakaran, J. R. Venugopal and S. Ramakrishna, Biomaterials, 2009, 30, 4996–5003 CrossRef CAS PubMed.
  63. G. Jin, M. P. Prabhakaran and S. Ramakrishna, Acta Biomater., 2011, 7, 3113–3122 CrossRef CAS PubMed.
  64. X. Yang, K. Zhao and G. Q. Chen, Biomaterials, 2002, 23, 1391–1397 CrossRef CAS PubMed.

This journal is © The Royal Society of Chemistry 2017