In this paper, we investigated the internal structure and the volume phase transition (VPT) behavior of poly(N-vinylcaprolactam-co-vinylimidazole)/polymerizable carbon nanodot (P(VCL-co-VIM)/PCND) microgels with different amounts of PCNDs. Our study shows that compared to the pure P(VCL-co-VIM) microgel, the hybrid microgels undergo a two-step VPT as the temperature increases and a core–shell(–corona) structure of the hybrid microgels is formed by copolymerization with PCNDs. A change in the amount of PCNDs has effects on both of the volume phase transition temperature and internal structure of microgels. Moreover, based on FT-IR in combination with perturbation correlation moving window (PCMW) and two-dimensional correlation spectral (2Dcos) analyses, the difference in VPT behavior between the shell and the core (corona) structure of the hybrid microgels at the molecular level is elucidated. The core/shell of the hybrid microgels fixed with hydrophilic PCNDs has a higher transition temperature during heating and a more compact structure due to the additional crosslinkers PCNDs.
As an alternative, carbon nanodots (CNDs) are another important class of fluorescent nanomaterials which are very suitable for biomedical applications due to their low toxicity, good water dispersibility and photostability.26 Herein, we develop a facile route to prepare core–shell and core–shell–corona structured PVCL-based microgels by copolymerization with vinyl-functionalized CNDs (PCNDs). A series of PVCL/PCND hybrid microgels with different amounts of CNDs were synthesized. Due to the difference in reactivity between VCL and PCNDs, we obtained microgels with a heterogeneous structure, i.e. a dense PVCL/PCND hybrid core and a loose PVCL-rich shell.
Recently, transverse relaxation nuclear magnetic resonance measurements have been utilized to investigate the structure and composition of microgels.27–29 However, it is difficult for 1H NMR to trace the changes in other non-proton chemical groups, such as the ester group. In this case, we need to take advantage of FTIR measurements. In addition, hydrogen bonding is proved to be of great importance for the delicate balance between hydrophobic and hydrophilic interactions in microgels. The polymer–water hydrogen bonds are dominant below the VPTT, leading to the swelling of microgels. During heating above the VPTT, the polymer–water hydrogen bonds break gradually and hydrophobic interactions dominate resulting in the collapse of microgels. It is commonly recognized that FTIR is a suitable method for studying the behavior of the core and the shell during the volume phase transition as the characteristic peaks of the core and shell can be identified and separately studied in the IR spectra.30,31 Therefore, in this work, we additionally attempted to use spectral methods to distinguish the specific roles of the inner core and outer shell of the PVCL/PCND hybrid microgels during the volume phase transition process. Two advanced spectral analysis techniques based on FTIR, perturbation correlation moving window (PCMW) and two-dimensional correlation spectroscopy (2Dcos), were also employed to detect the subtle information on microscopic variations of delicate interactions in the PVCL-based microgels during the VPT process, and with it, the relationship between the structure and the thermosensitive behavior of the core–shell PVCL-based microgels at the molecular level was elucidated.
CH2 end in the vinyl segments of the PVIM portion.33 Compared to the absorption band at 3110 cm−1 for free VIM, the observed shift to a lower wavenumber suggests the formation of a polymeric structure.33 In addition, the IR peak at 1715 cm−1 (–COOR) and the band at 1558 cm−1 (amide II) of PCNDs can be seen in the IR spectra of PVCL/PCND hybrid microgels indicating the successful fixation of the PCNDs into the microgels.32
![]() | ||
| Scheme 1 Schematic illustration of the preparation of P(VCL-co-VIM)/PCND microgels containing different amounts of PCNDs. | ||
Fig. 1 shows the TEM images of PVCL-based microgels with different amounts of PCNDs. The average diameters of microgels determined by TEM are ca. 168, 85, and 338 nm for PVCL-0, PVCL-10% and PVCL-50%, respectively. In the TEM images, PCNDs appear as dark black spots. The images show that PCNDs are distributed uniformly inside the core of the PVCL-10% microgel, while for PVCL-50% some aggregation exists. In addition, the PVCL-50% microgel consists of a PVCL-based shell, in which the PCNDs are distributed uniformly, and a PVCL-based gel corona with much less PCNDs. It suggests that the hybrid microgel has a core–shell(–corona) structure, due to the higher reactivity of PCNDs compared to VCL during polymerization (Fig. S4, ESI†), leading to the faster consumption of PCNDs than VCL. Note that the cross-linker BIS and PCND reacted faster than VCL, suggesting that BIS and PCND located mainly in the core of PVCL-10%.
Fig. 2 shows the change in hydrodynamic diameters of microgels as a function of temperature. The VPTT of PVCL-0 is found to be 34 °C. A two-step VPT occurs at around 32 and 36 °C for PVCL-10% corresponding to the shell and core, respectively, as well as 32 and 38 °C for PVCL-50% corresponding to the corona and shell, respectively. Two different transition temperatures are observed for both the hybrid microgels suggesting the distinct structures between the inner core and shell from their outer layer. The higher VPTT of the hybrid microgels should come from the incorporation of hydrophilic PCNDs in the core of PVCL-10% or the shell of PVCL-50%.34,35 As shown in Fig. S7 (ESI†), the hydrodynamic diameters of PVCL-10% and PVCL-50% show good reversibility after 5 cycles of the heating–cooling process between 20 and 54 °C, suggesting their prospects for preparing thermosensitive sensors.
![]() | ||
| Fig. 2 Variation of the hydrodynamic diameters (Dh) of (a) PVCL-0, (b) PVCL-10%, and (c) PVCL-50% microgels. | ||
In addition, to explore the structure of the hybrid microgels, the fluorescence emission intensity (1 mg mL−1) was evaluated (Fig. S8, ESI†). The lower photoluminescence (PL) intensity of PVCL-50% compared to PVCL-10% may arise from the co-effect of two factors: first, the thicker corona of the PVCL-50% microgel would scatter more photons that come from the PCNDs inside the microgels; second, PCND-rich cores would lead to self-quenching. Moreover, the observed lower intensity of PVCL-50% was accompanied by a CND concentration-dependent PL red-shift due to the self-absorbing/excitation effect as the CND concentration increased.
These findings are in line with our observations that the PVCL-50% microgel consists of a PCND-rich core, a PVCL/PCND hybrid shell and a PVCL-rich corona, and the PVCL-10% microgel has a relatively large PVCL/PCND hybrid core surrounded by a thinner PVCL-rich shell.
O stretching, 1645–1570 cm−1) which can be used to trace nearly all thermoresponsive group motions of the PVCL-based microgels. We can find that all the C–H stretching bands shift to lower wavenumbers as the temperature increases, while C
O exhibits a binary spectral intensity change in all the three microgels. The variations in C–H stretching bands can be interpreted as the hydrophobic hydration of C–H groups with neighboring water molecules. As reported, a higher number of water molecules surrounding C–H groups would lead to a higher vibrational frequency.36 In this case, we can conclude that all the C–H groups of the three microgels undergo dehydration upon heating. On the other hand, the amide I region consists of two parts: hydrogen bonded and free C
O, corresponding to the lower frequency and the higher one, respectively. Therefore, the variations of amide I groups upon heating can be explained by the transformation of hydrogen bonded carbonyls with water to free carbonyls. Based on this point, the three microgel systems have similar spectral change tendencies in the VPTs, and during heating water molecules are expelled outside leading to the collapse of microgel networks.
![]() | ||
| Fig. 3 Temperature-dependent FTIR spectra of the three P(VCL-co-VIM)/PCND microgels in D2O (10 wt%) during heating from 23 to 54 °C with an increment of 1 °C, respectively. | ||
To quantitatively evaluate the impact of temperature on the hydration status of different chemical groups during the VPTs of the three kinds of microgels, the temperature-dependent frequency shifts of νas(CH2) and the integral area changes of C
O were plotted, as presented in Fig. 4. The wavenumbers of the C–H groups of the three microgels show a sharp shift around VPTTs and a gradual shift above VPTTs, a typical asymmetric sigmoid curve. The changes in amide I during the heating process result from the transformation of hydrogen bonded C
O with water to free C
O, reflected by the emergence of characteristic bands for free C
O in PVCL-based microgels after volume phase transition. For the hybrid microgels, the initial shrinkage causes a continuous increase in the number of free carbonyls before turning points at ∼33 °C, which is approximate equal to the VPTT of PVCL-0. This thermal transition behavior should correspond to the gradual dehydration of the C
O groups in the shell of the PVCL-10% microgel and the corona of the PVCL-50% microgel, since the outer layer of both the hybrid microgels has a structure similar to that of the PVCL-0 microgel. With further increase in the temperature, sharp changes occur at 35 and 38 °C for PVCL-10% and PVCL-50%, respectively, when more water molecules are expelled outside the microgels. The second transition points reveal that the hybrid microgels contain another form of the PVCL-based network architecture that should be distinct from their outer layer. It also fits our previous speculation that the core of the PVCL-10% microgels and the shell of the PVCL-50% microgels are fixed with hydrophilic PCNDs resulting in a higher transition temperature. It is noted that the transitions of the hydrated C–H groups are more continuous than those of the relative hydrophilic C
O groups in both the hybrid microgels. In other words, in the temperature range with the relatively flat curves of C
O groups, the C–H groups responds prior to C
O groups upon heating, indicating that the core in the PVCL-10% microgel and the shell in the PVCL-50% microgel would firstly undergo conformational changes and then start their dehydration process in solution. Note that the C–H groups of PVCL-10% undergo the highest degree of dehydration among the three microgels, while for the C
O groups, the degree of dehydration increases with the reduced concentration of PCNDs (Fig. S9, ESI†). The different effect of PCND concentration on the dehydration process of C
O and C–H groups may be attributed to the fact that C
O groups are more hydrophilic than C–H groups. The hybrid microgels with a higher concentration of PCNDs are more hydrophilic, leading to less dehydration of hydrophilic C
O. The change in C–H groups will be further discussed by following the 2Dcos analysis.
Fig. 5 shows the PCMW synchronous and asynchronous spectra of PVCL-0 and PVCL-10% to investigate the VPTs upon heating from 23 to 54 °C, respectively. For PVCL-50%, the PCMW spectra are presented in Fig. S10 (ESI†). For clarity, we plotted all the transition points and regions read from PCMW maps in Fig. S11 (ESI†). As mentioned above, the PVCL-10% microgel possesses a relatively dehydrated core and a loosely cross-linked shell and PVCL-50% has a relatively dehydrated shell and a corona with a lower cross-linking density. Thus, the dehydrated C–H groups of these two microgels have an obviously earlier response than the hydrated ones upon heating indicating that C–H groups located in the relatively dehydrated core of PVCL-10% or the shell of PVCL-50% are more sensitive to the temperature rise. Besides, the C
O groups of the hybrid microgels have two VPTTs, and the higher one correspond to the core of PVCL-10% or the shell of PVCL-50% fixed with PCNDs. To further investigate the core structure of the PVCL-50% microgel, we also drew the PCMW synchronous map of the C
O region of PCNDs fixed in it (Fig. S12, ESI†). Note that the PCNDs themselves have no thermal sensitivity, while they will undergo a dehydration process in response to the temperature rise under the influence of adjacent PVCL segments. It can be seen that the transition points with regard to the hydrated C
O groups of the PCNDs locate at 35 and 46 °C, which are in the transition regions of the hydrated and dehydrated states of the shell of PVCL-50%, respectively, indicating that the PCNDs undergo two dehydration processes during heating. In the first stage, the PCNDs that are fixed in the shell of PVCL-50% undergo dehydration (35 °C) prior to the shrinkage of the shell in the PVCL-50% microgel (38 °C). Such a behavior is reasonable if we consider that a reduction of the effective charge density of hydrolyzed amino groups in the PCNDs is a prerequisite for further shrinkage of the interior of the microgels.37 After the dehydration process of the shell finishes at about 47 °C upon heating, the network of the shell becomes compact and the innermost PCND-rich core begins to dehydrate (46 °C), driven by the squeezing effect to remove more water molecules. The present mechanism can be proved in the following 2Dcos analysis.
O groups, it reveals that the conformational change of the C–H groups occurs before the dehydration of the C
O groups during heating. For the vibrational modes of C–H groups, the symmetric stretching vibration changes prior to the asymmetric stretching vibration upon heating. The direction of the asymmetric stretching vibration is parallel to the chain axis, while that of the symmetric stretching vibration is vertical with respect to the chain axis as previously reported.39 Therefore, it is deduced that the side chains collapse prior to main chains during the conformational changing process. Such sequence order that is opposite to that of the PVCL-4VP microgels as we reported previously14 may be attributed to the effect of the conformational change of the PVIM segments in the side chains during the VPT. As discussed above, the VIM units tend to accumulate in the loosely crosslinked VCL-rich outer layer of the PVCL-based microgels. Therefore, we can conclude that with increasing temperature above the LCST, the VIM units in the shell turn toward the outside of the shrinking microgels due to its hydrophilic nature, and the adjacent PVCL segments are forced to adjust their hydrophilic and hydrophobic groups in the perpendicular direction by the rearrangement of the VIM units.
As for the hybrid microgels, the 2Dcos spectra of the PVCL-10% and PVCL-50% microgels during heating from 23 to 54 °C are shown in Fig. 6 and Fig. S14 (ESI†), respectively. In the C–H region of PVCL-10%, two distinct kinds of dehydrated C–H bands appear at 2926 and 2916 cm−1, respectively. The one at 2926 cm−1 is in accordance with PVCL-0, and the appearance of the lower one indicates that there exists another structure in PVCL-10% which is less hydrated than that in PVCL-0. As mentioned before, the C–H groups in the core of PVCL-10% are less dehydrated than the shell, thus we can attribute the new band at 2916 cm−1 to the C–H groups that are close to PCNDs in the core. Similarly, the C–H bands at 2960, 2943 and 2914 cm−1 detected in the asynchronous spectra of the PVCL-50% microgel can be assigned to less hydrated C–H groups neighboring PCNDs in the shell. For clarity, Table 1 and Table S2 (ESI†) list all the bands detected in the 2Dcos spectra and their tentative assignments, respectively. We can deduce the specific order for the heating process of PVCL-10% in D2O: 2916 → 1608 → 1618 → 1587 → 2950 → 2868 → 1632 → 2926 → 2858 cm−1. Regardless of the differences in stretching modes, we have C
O → C–H, indicating the phase transition is driven by the hydrogen bonding transformation of amide groups. It is interesting to note that the band at 2916 cm−1 which is attributed to the dehydrated C–H groups that are close to PCNDs shows an earlier response than all the bands during the VPT. This is because the fixed PCNDs with hydrophilicity will “attract” most water molecules in the core, and endow the inner core of PVCL-10% with a more compact network. As a result, the hydrophobic C–H groups in the core of PVCL-10% locate in a relatively hydrophobic environment and undergo a more efficient dehydration than those in the core of PVCL-0 during the VPTT, in line with the above conventional IR analysis. In addition, the order of the vibration modes for C–H groups in the PVCL-10% microgel is the reverse of that in the PVCL-0 microgel, and the backbones of the PVCL-10% microgel change prior to the side chains during heating. This may be attributed to the fact that the PCND-crosslinkers with an earlier dehydration process induce the changes in neighboring groups in the main chains prior to the ones in the side chains. In all, the VPT process of the PVCL-10% microgel begins from the relatively dehydrated core, and then the C
O and C–H groups associated with water molecules in the shell start to dehydrate. When the temperature increases above the VPTT of the core, which is higher than normal owing to the hydrophilic property of PCNDs, more water molecules are gradually squeezed out from the compact core.
| Wavenumber (cm−1) | Tentative assignments |
|---|---|
| 2950 | ν as(hydrated CH2) |
| 2926 | ν as(dehydrated CH2) |
| 2916 | ν as(dehydrated CH2, close to PCNDs) |
| 2868 | ν s(hydrated CH2) |
| 2858 | ν s(dehydrated CH2) |
| 1632 |
ν(free C O) |
| 1618 |
ν(C O⋯D–O–D⋯O C) |
| 1608 |
ν(C O⋯D–O–D) |
| 1587 |
ν(C O⋯(D–O–D)2) |
For the PVCL-50% microgel, the final sequence for the groups during heating is: 1606 → 1589 → 2968 → 2870 → 2960 → 2914 → 2950 → 2935 → 2852 → 2943 → 1618 → 1635 cm−1. One can see that the C–H groups close to PCNDs show a later response than the other C–H groups during the VPT. It could be explained by the higher VPTT of the shell where the C–H groups close to PCNDs are mainly distributed. From the overall sequence order, we can find that when the temperature reaches the phase transition temperature of the corona with a structure similar to that of PVCL-0, the hydrogen bonds formed between the C
O groups of PVCL and water will break, and then the main chains of PVCL start to collapse. Subsequently, with further increase in the temperature the less hydrated shell with a higher transition temperature begins to shrink and expels out water molecules. Combined with the PCMW analysis of PCNDs, water is forced to squeeze out of the hydrophilic PCND-core following the VPT process of the corona and shell finishing with more compact networks. For clarity, the VPTs of PVCL-0 and the two hybrid microgels during heating are illustrated in Scheme 2. PVCL-0 exhibits a typically thermal-sensitive behavior, which has a relatively sharp transition around the VPTT, while for the hybrid microgels, a two-step VPT upon heating can be observed, and the core of PVCL-10% and the shell of PVCL-50% with higher VPTTs dehydrate following the VPT process of their layer. Moreover, the core of PVCL-50% is forced to dehydrate after the dehydration of the shell.
![]() | ||
| Scheme 2 Schematic illustration and comparison of the VPTs of the PVCL-0, PVCL-10% and PVCL-50% hybrid microgels in water. The light blue color represents the distribution density of water molecules. | ||
O groups in conventional IR analysis, respectively. From this we can infer that the inner core or shell of the hybrid microgels has distinct structures and components from their outer layer and the higher transition points of the hybrid microgels come from the incorporation of the hydrophilic PCNDs in the core of PVCL-10% or the shell of PVCL-50%. The FLS measurements support the formation of the core of the PVCL-50% microgel by self-polymerization of the PCNDs. Moreover, in combination with the 2Dcos analysis, the C–H groups of PVCL-10% undergo the highest degree of dehydration among the three microgels, which can be attributed to the fact that the fixed PCNDs with hydrophilicity will “attract” most water molecules in the core and endow the inner core of PVCL-10% with a more compact network leading to a relatively hydrophobic environment for the hydrophobic C–H groups, thereby enabling them undergo more efficient dehydration than those of PVCL-0.
Footnote |
| † Electronic supplementary information (ESI) available: TEM images and 1H NMR spectra of PCNDs, fluorescence emission spectra of hybrid microgels, DLS curves of the hybrid microgels, IR spectra of PCNDs and hybrid microgels, experimental section and detailed description of PCMW and 2Dcos. See DOI: 10.1039/c6cp06862f |