Open Access Article
Xiangyu Tan‡
a,
Jiajun Du‡c,
Haitao Wuc,
Xuyu Mab,
Chunbo Zhoud,
Fangrong Zhoua,
Caijin Fane,
Xueqin Xud,
Shaocong Hou
*b and
Xin Cai
*c
aPower Science Research Institute of Yunnan Power Grid Co., Ltd., Kunming 650214, China
bSchool of Electrical Engineering and Automation, Wuhan University, Wuhan 430072, China. E-mail: sc.hou@whu.edu.cn
cCollege of Materials and Energy, South China Agricultural University, Guangzhou 510642, China. E-mail: caixin2015@scau.edu.cn
dQujing Power Supply Bureau of Yunnan Power Grid Co., Ltd., Qujing 655099, China
eState Key Laboratory of HVDC, Electric Power Research Institute, CSG, Guangzhou, 510080, China
First published on 18th September 2024
Developing high-efficiency interlayer catalysts is a promising tactic for improving the cycling performance of rechargeable lithium–sulfur (Li–S) batteries. Herein, using the Prussian blue analogue as the precursor, cobalt–zinc carbide nanocrystal-embedded N-doped porous carbon (Co3ZnC@NC) is synthesized via simple post-carbonization. The obtained Co3ZnC@NC nanospheres exhibit a robust core–shell structure showing good conductivity, high porosity and available metal active sites, favoring the interfacial charge transfer and the electron transport upon electrochemical reactions. The results demonstrate that the Co3ZnC@NC catalyst is quite suitable for boosting the adsorption and redox conversion kinetics of soluble polysulfides. When acting as the separator interlayer, Co3ZnC@NC contributes to improved Li–S batteries with a high discharge specific capacity of 1659.8 mA h g−1 at 0.1C and superior cycling stability of over 250 cycles at 1.0C (high capacity retention of 84.1% after 100 cycles at 0.5C). Furthermore, the Co3ZnC@NC-based battery can maintain a high discharge capacity of 734.0 mA h g−1 at 5.0C, along with delivering a stable reversible capacity of 805.4 mA h g−1 (∼5 mA h cm−2) after 50 cycles even under a high sulfur loading of 6.2 mg cm−2. This study affords a viable way to construct highly dispersed bimetal/carbon composites for efficient catalysts and renewable energy devices.
To inhibit the shuttling effect of LiPSs for improved Li–S batteries, tremendous efforts have been made to elucidate the reaction mechanism of Li–S electrochemistry.9 Thus, designing suitable high-activity electrocatalysts has become a primary option that can speed up the slow reaction kinetics of lithium polysulfides involving a complex multi-electron transfer process.10 As an indispensable part of the electrochemical energy device, the separator could play a crucial role in modulating the complicated “solid–liquid–solid” interfacial reactions during lithium storage, thus largely impacting the performance of Li–S batteries.11 Accordingly, modifying commercial separators with functional interlayer electrocatalysts has been a feasible strategy for promoting battery performance.12 Those functional separators can generally mitigate LiPS shuttling by trapping the dissolvable LiPSs at the cathode side and effectively reducing the corrosion of the lithium anode.13 Among diverse interlayer catalysts, various porous carbon materials have been adopted to obtain functional separators, limiting the shuttle of polysulfides by physically blocking the LiPSs with abundant and appropriate pores.14 Taking advantage of electronegative heteroatom (e.g. N, S, and P) doping, the physical adsorption and binding ability of the carbon surface toward the LiPSs can be increased.15 However, the chemical affinity and electrochemical properties of most carbon catalysts toward sulfur electrocatalysis are still restricted, leaving sufficient room to improve the cycling capacities and the long-term stability of corresponding Li–S batteries.16
To address these issues, polar metal compounds (e.g. sulfides, nitrides, oxides and phosphides of non-precious metals) with strong chemical affinity and abundant electroactive sites are introduced as catalysts for boosting the sluggish redox conversion of LiPSs at the multiphase interfaces.17–19 By rationally hybridizing metal compounds with porous carbon matrix, desirable catalysts with good conductivity, high selective permeability and excellent electrocatalytic activities can be achieved.20–23 Such hybridized catalysts are promising to use fully the synergistic effects between the porous carbon nanostructure and the metal active sites, which considerably accelerates the adsorption and catalytic conversion of LiPSs during reversible battery reactions.24,25 Intriguingly, transition metal carbides have attracted much attention in (electro-)catalytic fields due to their electroactivity, prominent electronic conductivity, high stability and good compatibility with carbon supports.26–28 By constructing desired transition metal carbide-based hybrid catalysts, one major challenge is to ensure homogeneously dispersed and sufficient metal active sites in the carbon matrix.29 Moreover, the different valence changes in the metal centers are often conducive to manipulating the charge transfer as well as the adsorption/desorption behavior between the active sites and the LiPS intermediates, which ultimately influence the redox kinetics of Li–S electrochemical reactions.30,31 In early 2016, Wang et al. hybridized exfoliated-metal carbide (Ti3C2Tx) nanosheets with mesoporous carbon to host sulfur. Profiting from the effective trapping of sulfur and polysulfides by metal carbides, the sulfur cathode contributed to improved Li–S batteries with a discharge capacity of 1225.8 mA h g−1 and stable cycling of over 300 cycles at 0.5C.32 Zhang et al. used nitrogen-doped carbon-supported Co3Mo3C to modify the commercial separator. The results demonstrated that bimetallic Co3Mo3C could provide more binding sites for polysulfide adsorption and catalysis compared with monometallic Mo2C, thus leading to highly stable Li–S batteries with greatly increased sulfur utilization.33 Hong et al. proposed Ni3ZnC0.7/Ni/NCNTs-functionalized separators for high-performance Li–S batteries with excellent rate capabilities. The study illustrated the advantageous properties of the bimetal carbides with sulfophilic Ni sites and lithophilic Zn sites to regulate the redox kinetics of polysulfides.34 Despite this encouraging progress, it is still essential to develop high-efficiency bimetal carbide-based interlayer catalysts through simpler, low cost, and scalable syntheses to better increase sulfur utilization toward practical Li–S batteries.35
In consideration of the above, in this work, we designed nitrogen-doped porous carbon-encapsulated cobalt–zinc carbides (Co3ZnC@NC) nanospheres through a simple one-pot synthesis. The Co3ZnC@NC composite was derived from the post-carbonization of the Prussian blue analogue precursor. Benefiting from the core–shell structure that comprises highly dispersed bimetal carbide nanocrystals and thin N-doped carbon shells, Co3ZnC@NC was endowed with hierarchical pores, good conductivity and abundant metal catalytic sites. Experimental results demonstrated the key role of Co3ZnC@NC in boosting the adsorption and reversible catalytic conversion of LiPSs during electrochemical reactions. By modifying the commercial polypropylene separator with Co3ZnC@NC, corresponding rechargeable Li–S batteries achieved high discharge capacities (1144.6 mA h g−1 at 0.5C), superior cyclic stability (long cycling of over 250 cycles at 1.0C) and good high-rate performance (734.0 mA h g−1 at 5.0C), showing inhibited shuttling of polysulfides upon charge/discharge cycling.
:
1
:
1, respectively, while N-methylpyrrolidone (NMP) was used as the solvent and stirred for 12 h to obtain a uniform mixture. Then, the resulting slurry was coated onto one side of the commercial separator (Celgard 2500) by applying the doctor blading method. The modified separators were then dried overnight in a vacuum oven at 60 °C, generating the Co3ZnC@NC/PP separators. Typically, Co3ZnC@NC/PP separators were cut into 19 mm discs with a catalyst loading amount of approximately 0.8 mg cm−2. In comparison, the Super P modified separator (Super P/PP) was prepared according to the same procedures without incorporating Co3ZnC@NC.
:
1 for 15 min, and then placed into a tube furnace. The powder was heated at 155 °C for 12 h under N2 atmosphere and further sublimated at 200 °C for 30 min at a heating rate of 2 °C min−1. The sample collected after cooling was the active carbon/sulfur composite. The preparation of the sulfur cathode pieces was as follows. 80 wt% of the carbon/sulfur composite, 10 wt% of Super P and 10 wt% of the LA133 binder (5 wt% in water) were evenly mixed with deionized water and fully stirred in deionized water for 12 h, and the acquired slurry was uniformly coated onto the carbon-coated side of aluminum foil using the doctor blading method. As-fabricated cathode pieces were dried overnight in a vacuum oven at 60 °C and finally cut into cathode discs with a diameter of 12 mm and a specific sulfur loading of 1.2–1.3 mg cm−2.
:
DOL = 1
:
1 vol%) by incorporating 1.0 wt% lithium nitrate (LiNO3) as the additive. For the assembly of symmetrical cells, two identical Co3ZnC@NC-based electrodes acted as the working electrode and the counter electrode, respectively. A commercial separator (PP, Celgard 2500) was used as the separator, and the electrolyte (20 μL) was composed of 0.2 mol L−1 Li2S6, 1.0 M LiTFSI and 1.0 wt% LiNO3 in the mixed solvent of DME and DOL (vDME/vDOL = 1
:
1).![]() | ||
| Fig. 1 (a) Schematic preparation of the Co3ZnC@NC composite, (b) XRD patterns of different samples, and (c) thermogravimetric curve of Co3ZnC@NC. | ||
SEM images of the as-synthesized composite are shown in Fig. 2a and b. It can be observed that Co3ZnC@NC is basically composed of relatively dispersed and uniform nanoparticles. Some of these densely packed nanoparticles are connected by a few short carbon nanotubes (Fig. 2c), which is not uncommon because the presence of active cobalt-based species can often catalyze the growth of carbon nanotubes under high-temperature carbonization.36 The fine structure of Co3ZnC@NC is illustrated in Fig. 2d, revealing that Co3ZnC@NC mainly comprises irregular nanoparticles with particle sizes of 30–50 nm. According to Fig. 2e and f, Co3ZnC@NC demonstrates a typical core–shell nanostructure, where the internal Co3ZnC nanocrystals are stably surrounded by thin N-doped carbon shells. Moreover, the lattice spacing of the inner nanoparticles is about 0.217 nm and 0.264 nm, corresponding to the characteristic (110) and (111) faces of the Co3ZnC nanocrystals. Fig. 2g–l displays the energy disperse spectroscopy (EDS) mapping images of Co3ZnC@NC, showing that Co, Zn, C, N, and O elements are homogeneously distributed in the core/shell structured nanoparticles. Obviously, Co and Zn species are dominantly concentrated in the core of the nanoparticle, while C and N elements exhibit aggregated distribution in the outer layer of the nanoparticle along with apparent spreading over the entire nanoparticle. Unavoidably, the uniform distribution of O element in the composite is reasonable because many active nanocarbon or metal nanoparticles often endure slight oxidation to introduce oxygen-containing groups on the surfaces upon synthesis and utilization.37 All the above results confirm the effective hybridization of Co3ZnC nanocrystals and N-doped carbon to form core–shell structured Co3ZnC@NC.
Fig. 3a demonstrates the N2 adsorption/desorption isotherms of Co3ZnC@NC. The BET surface area of Co3ZnC@NC is determined to be 53.40 m2 g−1. Thus, the pore volume of the Co3ZnC@NC composite is 0.202 cm3 g−1 with an average pore size of 16.26 nm. The pore size distribution reveals that Co3ZnC@NC is characterized by a hierarchical structure consisting of considerable micropores and sufficient mesopores. These hierarchical pores can ensure the appropriate penetration of the electrolyte into the catalyst to improve ion diffusion. Moreover, more exposed active sites are available to positively anchor/adsorb the soluble LiPSs to accelerate the catalytic conversion rate of LiPSs38 to confine the LiPSs at the cathode reaction interfaces with reduced shuttling effect.
![]() | ||
| Fig. 3 (a) Nitrogen adsorption/desorption curves and pore size distribution (inset) of Co3ZnC@NC; Co 2p (b), Zn 2p (c), C 1s (d), N 1s (e) and O 1s (f) spectrum of Co3ZnC@NC. | ||
To investigate the surface chemical composition and electronic state of the Co3ZnC@NC catalyst materials, X-ray photoelectron spectroscopy (XPS) characterization was performed. The full spectrum further verified the coexistence of the main characteristic peaks of C 1s, N 1s, O 1s, Co 2p, and Zn 2p. The contents of C, N, O, Co, and Zn elements on the surface of Co3ZnC@NC were 74.32%, 12.69%, 8.31%, 1.35% and 3.33%, respectively. Fig. 3b shows the high-resolution Co 2p spectrum of Co3ZnC@NC. The pair of sharp peaks at 778.1 and 793.1 eV can be ascribed to the characteristic Co0 species, suggesting the adequate proportion of metallic Co present in the bimetal carbides under pyrolysis. This result agrees well with the above-mentioned observation that minor carbon nanotubes were generated by Co-catalyzed growth during the carbonization synthesis of Co3ZnC@NC.39 The prominent peaks at 778.8 and 793.7 eV correspond to the Co2+ species, along with two satellite peaks occurring at 781.9 and 796.8 eV. It is rational that the coexistence of Co0 and Co2+ could effectively balance the valence states of Co active sites, which is beneficial for enhancing the chemical adsorption and targeted anchoring of LiPSs by the active electrocatalyst during battery reactions.35 In the high-resolution Zn 2p spectrum (Fig. 3c), two featured peaks at 1021.8 and 1044.9 eV can be assigned to Zn2+. Previous findings have illustrated that the presence of a second metal species (e.g. Zn2+) can cooperate with Co2+ to act as a reservoir, achieving synergistic adsorption and catalytic conversion of LiPSs.40,41 For the C 1s spectrum illustrated in Fig. 3d, the diffraction peaks are C–C (284.8 eV), C–N (285.7 eV) and C
O (288.3 eV), indicating that the carbon layer on the surface of Co3ZnC@NC is rich in abundant C–N bonding. Such electronegative nitrogen-rich carbon coating can introduce more disordered defects, increase the surface chemical affinity of the Co3ZnC@NC composite toward LiPSs, and stabilize the internal bimetal carbides nanocrystals upon electrochemical cycling. According to Fig. 3e of the N 1s spectrum, the peak corresponds to pyridinic N (398.3 eV), pyrrolic N (400.5 eV), graphitic N (401.1 eV) and N oxides (403.5 eV). Conformably, the apparently high content of pyridinic N and pyrrolic N promoted electron transfer on the surface of the hybrid electrocatalyst, favoring the redox reactions of long-chain LiPSs.42 For the O 1s spectrum (Fig. 3e), the C–O bond at 531.1 eV and the C
O bond at 532.2 eV further infer the partial oxidation on the surface of Co3ZnC@NC.
Fig. 4a shows the UV-vis absorption curves and corresponding optical photos of different samples after the static adsorption of Li2S6. Compared to Super P and the blank samples, Co3ZnC@NC exhibited obviously increased adsorption capacity and high trapping ability toward polysulfides, which can be verified by the cleared color and the almost disappeared characteristic peaks of the Li2S6 solution in the UV-vis absorption spectrum.25 To verify the electrocatalytic performance of Co3ZnC@NC for LiPSs, cyclic voltammetry (CV) tests of symmetric cells were performed with Li2S6 solution as the electrolyte across the operating voltage range of −1.0 V to 1.0 V. In addition, a control cell using an electrolyte without Li2S6 was investigated as the reference. As shown in Fig. 4b, the reference cell basically produces a negligible current contribution, while the symmetric cell containing Li2S6 exhibits obvious current response and significant redox peaks at −0.06 V and 0.06 V, indicating the adorable electrochemical properties of the Co3ZnC@NC composite for catalyzing the redox conversion of soluble LiPSs.
To further examine the electrochemical performance of the designed catalyst in actual batteries, Co3ZnC@NC was used as an interlayer catalyst to modify the commercial PP separator, obtaining the Co3ZnC@NC/PP-based Li–S battery. Unless otherwise mentioned, all the assembled Li–S batteries adopted a cathode with a sulfur loading of 72 wt% (Fig. S1†). Fig. 4c shows the Nyquist plots of fresh batteries based on Co3ZnC@NC/PP and PP separator through electrochemical impedance spectroscopy (EIS) characterization. It is reasonable that the entire internal resistance of the battery significantly decreases after the involvement of Co3ZnC@NC. Thus, the charge transfer resistance (Rct) of the Co3ZnC@NC/PP battery (24.2 Ω) is much smaller than that of the PP battery (47.5 Ω), suggesting that the Co3ZnC@NC interlayer catalyst can dramatically improve the interfacial charge-transfer by simultaneously providing sufficient electrocatalytic sites and a good conductive network, leading to accelerated redox kinetics of sulfur species, especially on the cathode side of the battery.43,44 Moreover, the redox reaction process of Li–S batteries was investigated in the operating voltage range (1.7–2.8 V) using CV at a low sweep rate of 0.1 mV s−1. As shown in Fig. 4d, two separate reduction peaks centered at 2.34 and 2.05 V appear in the cathodic sweeping process, while two distinct peaks (2.3–2.5 V) in the anodic sweeping process can be observed. The former results from the stepwise production of long-chain Li2Sn (4 ≤ n < 8) and short-chain polysulfides (1 ≤ n < 4) by reducing the elemental sulfur.45 The latter corresponds to the backward oxidation of lithium sulfide to Li2Sn (2 ≤ n ≤ 8). With the incorporation of Co3ZnC@NC, the relevant battery delivers much stronger peak currents and reduced polarization potentials. It can be concluded that Co3ZnC@NC exhibits a superior catalytic ability to facilitate reaction kinetics and improve the redox conversion of LiPSs during the battery charge/discharge process. Moreover, CV tests were performed on the PP battery and Co3ZnC@NC/PP battery under different scanning rates. As demonstrated in Fig. 4e, the peak current and electrode polarization of the Li–S battery gradually increase as the scanning rate increases. Using the Randles–Sevcik equation, we analyzed the relationship between the peak current (Ip) of the characteristic redox peaks and the square root of the scanning rate (v0.5).46 As displayed in Fig. 4f, there is a certain linear relationship between Ip and v0.5. In particular, the lithium ion diffusion coefficients (DLi+) of peaks A, B and C are calculated to be 1.59 × 10−7, 0.64 × 10−7 and 5.91 × 10−7 cm2 s−1, respectively, which are obviously higher than those of the PP battery (Fig. S2 and S3†), further confirming the favorable ion transport and electrochemical reversibility by the Co3ZnC@NC catalyst. Notably, the DLi+ of the oxidation peak is significantly higher than the others. This infers that Co3ZnC@NC could behave better at the catalytic conversion of short-chain Li2Sn to long-chain LiPSs rather than the opposite reduction pathway.47
Fig. 5a shows the cycling performances of Li–S batteries based on Co3ZnC@NC/PP, Super P/PP and PP separator under a current density of 0.5C. Compared to the other two counterparts, the Co3ZnC@NC/PP exhibits extremely improved discharge capacities and cycling stability. In particular, the initial discharge specific capacity of the Co3ZnC@NC/PP battery is 1144.6 mA h g−1 higher than that of Super P/PP (1003.6 mA h g−1) and PP battery (635.1 mA h g−1). After 100 continuous charge/discharge cycles, the Co3ZnC@NC/PP battery can maintain a high discharge capacity of 962.6 mA h g−1, yielding a retention rate of 84.1%, which is superior to that of the Super P/PP (79.6%) and PP battery (61.6%) with much lower retention capacity. Moreover, the high coulombic efficiencies of the Co3ZnC@NC/PP battery during cycling demonstrate its excellent reversibility and durability during charge/discharge reactions.48,49 Correspondingly, the initial galvanostatic charge–discharge curves of batteries with different separators are compared, as depicted in Fig. 5b, which magnifies the relatively low electrode polarization of the Co3ZnC@NC/PP battery. Further, after 100 successive cycles, the electrode polarization of the Co3ZnC@NC/PP battery did not change much (Fig. 5c). This suggests that the Co3ZnC/NC interlayer catalyst can effectively improve the electrochemical reversibility and capacity performance of Li–S batteries. According to the S 2p spectrum of Co3ZnC@NC after cycling at 0.5C for 50 cycles (Fig. S4a†), the prominent Co–S bonding further infers the strong chemical affinity and anchoring ability of Co3ZnC@NC toward polysulfides. Moreover, the evident negative shift of the N 1s peaks along with the positive shifts of both Co 2p peaks and Zn 2p peaks indicates the redistributed electron density of the metal centers or the metal–N moieties (Fig. S4b–d†), which could act as active sites for enhanced polysulfide interaction and catalytic conversion.
The rate performance of the Li–S batteries is demonstrated in Fig. 5d. Co3ZnC@NC/PP-based battery delivers a specific discharge capacity of 1659.8 mA h g−1 at 0.1C. As the current density incrementally increases to 0.2C, 0.5C, 1.0C, 2.0C, 3.0C and 5.0C, the corresponding specific capacity is 1246.9, 1136.7, 1047.3, 918.4, 823.4 and 734.0 mA h g−1, greatly surpassing that of the PP battery. Then, when the current density returns to 0.2C, the discharge specific capacity can still be restored to 1201.7 mA h g−1 for the Co3ZnC@NC/PP battery. This indicates that the active sites of the Co3ZnC@NC composite can achieve stable adsorption and electrocatalytic promotion of LiPSs upon lithium storage at different current densities, thus contributing to the high specific capacities and excellent rate capability of the battery at high rates. Based on the charge–discharge curves illustrated in Fig. 5e and f, the increases in the voltage gap of the Co3ZnC@NC/PP battery are significantly smaller than those of the PP battery at different current densities, further proving the efficient utilization of active sulfur and superb cycling stability by involving the Co3ZnC@NC interlayer as a polysulfide mediator in Li–S batteries during battery operation.
Furthermore, the long-term cyclic stability of the designed Li–S batteries was investigated. As presented in Fig. 6a, the Co3ZnC@NC/PP-based battery delivers an initial discharge capacity of 996.6 mA h g−1 at 1.0C. After 250 charge/discharge cycles, the battery can well maintain a reversible specific capacity of 695.8 mA h g−1, exhibiting capacity retention of 69.8% and an average decay rate per cycle of about 0.121%. Additionally, the coulombic efficiencies of the battery are stably above 96%. The results demonstrate the distinctly enhanced battery stability and excellent cycling performance by the Co3ZnC@NC-modified functional separator upon long cycling. When the sulfur loading of the cathode was drastically elevated to 6.2 mg cm−2 (i.e. E/S of 6 μL mg−1), the corresponding Co3ZnC@NC/PP battery can maintain a high discharge capacity of 805.4 mA h g−1 (areal capacity of ∼5 mA h cm−2) at 0.2C (Fig. 6b) and 542.8 mA h g−1 at 0.5C (Fig. 6c) even after 50 continuous cycles, shedding light on its superior cycling stability and promising practical potential toward high-specific energy output with lean electrolyte (Table S1†).
To further elucidate the positive role and key electrocatalytic performance of the Co3ZnC@NC/PP catalyst for the redox conversion of LiPSs, typical nucleation/dissolution experiments were performed by assembling the coin battery with the Co3ZnC@NC electrode and the Li2S8-contained electrolyte.50,51 Fig. 6d illustrates the potentiostatic discharge current–time plot of Co3ZnC@NC at an operating voltage of 2.05 V. The specific capacity of the Co3ZnC@NC electrode toward Li2S nucleation is calculated to be 111.28 mA h g−1. Furthermore, by fitting the charging current–time plot of the Co3ZnC@NC electrode operating at 2.40 V, a high specific capacity of 409.19 mA h g−1 is achieved for Co3ZnC@NC toward Li2S dissolution (Fig. 6e). The relatively adorable nucleation/dissolution ability of Li2S strongly confirms the chemical affinity and superior catalytic activity of the functional Co3ZnC@NC layer. Co3ZnC@NC could dominantly inhibit polysulfide shuttling by facilitating the interfacial charge transfer process and reducing the activation barrier for the phase nucleation of polysulfides52,53 to achieve accelerated redox kinetics of LiPSs and improved sulfur utilization of correlated Li–S batteries.
Footnotes |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ra04657a |
| ‡ Xiangyu Tan and Jiajun Du contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2024 |