Sofia
Martins
*a,
Zheng
Ma
a,
Xavier
Solans-Monfort
b,
Mariona
Sodupe
b,
Luis
Rodriguez-Santiago
b,
Enric
Menéndez
a,
Eva
Pellicer
*a and
Jordi
Sort
ac
aDepartament de Física, Universitat Autònoma de Barcelona, E-08193 Cerdanyola del Vallès, Spain. E-mail: CarlaSofia.Martins@uab.cat; Eva.Pellicer@uab.cat
bDepartament de Química, Universitat Autònoma de Barcelona, E-08193 Cerdanyola del Vallès, Spain
cInstitució Catalana de Recerca i Estudis Avançats (ICREA), Pg. Lluís Companys 23, E-08010 Barcelona, Spain
First published on 25th November 2022
Electric-field-driven ion motion to tailor magnetic properties of materials (magneto-ionics) offers much promise in the pursuit of voltage-controlled magnetism for highly energy-efficient spintronic devices. Electrolyte gating is a relevant means to create intense electric fields at the interface between magneto-ionic materials and electrolytes through the so-called electric double layer (EDL). Here, improved magneto-ionic performance is achieved in electrolyte-gated cobalt oxide thin films with the addition of inorganic salts (potassium iodide, potassium chloride, and calcium tetrafluoroborate) to anhydrous propylene carbonate (PC) electrolyte. Ab initio molecular dynamics simulations of the EDL structure show that K+ is preferentially located on the cobalt oxide surface and KI (when compared to KCl) favors the accumulation of positive charge close to the surface. It is demonstrated that room temperature magneto-ionics in cobalt oxide thin films is dramatically enhanced in KI-containing PC electrolyte at an optimum concentration, leading to 11-fold increase of generated magnetization and 35-fold increase of magneto-ionic rate compared to bare PC.
New conceptsVoltage control of magnetism (VCM) through electric field-induced ion motion, referred to as magneto-ionics, is a cutting-edge research topic since it holds the promise to revolutionize current strategies to enhance energy efficiency in magnetically actuated devices (e.g., micro-electro-mechanical systems, magnetic logics, spintronics, or neuromorphic computing). Modifying the film composition/microstructure or the working conditions are the typical approaches followed in the literature to boost magneto-ionics. However, at present, room temperature oxygen magneto-ionics is still too slow for relevant applications. Increased O2− motion speeds and smaller threshold voltages are highly desirable. Here, we demonstrate that O2− motion in electrolyte-gated cobalt oxide films can be significantly enhanced by suitable ‘electrolyte engineering’ in films of a few nm in thickness. In particular, inorganic salts (e.g., KI, KCl and (Ca(BF4)2), have been added to anhydrous propylene carbonate (PC) to modulate the ionic strength and, in turn, the electric field at the cobalt oxide/electrolyte interface by means of the built-in electric double layer. For KI-containing PC, a 35-fold increase of the magneto-ionic rate is observed compared to plain PC and, importantly, under a relatively low bias value (<−1.5 V), much lower than the voltage values needed so far to induce magneto-ionics in this kind of systems. |
Electrolyte-gating through the formation of an electric double layer (EDL) has shown to be a very convenient means to tailor the magnetic properties of magneto-ionic systems. These systems work as electrochemical capacitors (EC), i.e., supercapacitors, thereby involving the formation of an EDL between the solid material and the electrolyte. At least three types of ECs can be distinguished, namely electrical double layer capacitors (EDLC), pseudocapacitors, and a combination of both.5,6 Whatever the type, ECs refer to a system capable to accumulate electrical charges at the surface of an electrode material in contact with an electrolyte. When voltage is applied to a magneto-ionic material, the electric field causes changes in its saturation magnetization (MS) or coercivity (HC), among other magnetic properties, which can be finely tuned based on electrostatic and/or electrochemical mechanisms.7,8
According to the different models put in place to explain the concept of EDLs formed at the interface between planar solids and aqueous solutions, the simplest theory states that EDLs form to neutralize the surface charge on the solid material by ions of opposite sign (Helmholtz model). The more elaborated Gouy–Chapman–Stern model (GCS) is currently widely used to describe EDLs. It assumes the occurrence of two layers, one fixed layer next to the electrode surface (Stern layer or Helmholtz region) of opposite charge, and a diffuse layer, wherein ions can move freely. The Stern layer, in turn, is divided into the inner Helmholtz plane (IHP) and the outer Helmholtz plane (OHP). The former has approximately one single ion thickness. Compared to aqueous solutions, studies on the structure of EDL in organic solvents are more limited. Feng et al. examined a system made of tetraethylammonium tetrafluoroborate (TEABF4) salt in acetonitrile (CH3CN) and found remarkable contact adsorption of TEABF4 ions to the surface of the electrode and strong layering and orientational ordering of acetonitrile molecules until approx. 1.1 nm into the bulk electrolyte.9 The EC based on interfacial ion-modulation has attracted much interest because of the giant charge-carrier density accumulation achieved because of the large EDL capacitance. Under electrolyte gating, permanent changes at the surface and the bulk of electrode material are possible, whenever chemical reactions are involved.
Materials such as carbon, metal oxides and nitrides, and conducting polymers have been used in an EC.5,6 Metal oxides/nitrides such as Co3O410–12 and CoN13,14 are very appealing for magneto-ionics, since they not only store energy like electrostatic carbon materials but can also undergo electrochemical reactions under voltage actuation, eventually leading to a fully reversible transformation from a paramagnetic state (OFF) to a ferromagnetic state (ON), and vice versa. This is explained by oxygen and nitrogen motion, respectively, under voltage actuation, the concurrent creation of atomic defects, and the consequent generation of magnetic moment arising from metallic Co.10–14
The maximum electric field achievable in ECs is limited by the breakdown voltage of the electrolyte. Four primary classes of electrolyte solutions have been used in EC: organic, aqueous, polymeric and ionic liquid electrolytes. Among organic electrolytes, ACN and propylene carbonate (PC) are the most widely used solvents. ACN presents the ability to solvate large amounts of salts but it is toxic, while PC is more environmentally friendly, offers a wide electrochemical window and operating temperature, as well as conductivity of 1–2 × 10−8 Ohm−1 cm−1.5,15,16 Indeed, PC is a dipolar protic solvent with high dielectric constant (64.40 at 25 °C) and a large dipole moment (4.81 D) which has been considered an ideal structureless dielectric to solubilize strong electrolytes for a variety of applications. Since PC has a relatively large dielectric constant, dissolved ionic compounds will be extensively dissociated.
In spite of the achievements with VCM of Co oxide films, room temperature magneto-ionics is still too slow for relevant applications. Even though sub-10 s magneto-ionics has recently been demonstrated by reducing the Co oxide thickness down to 5 nm,12 further improvements are required to enable magneto-ionics in real devices. In addition, the applied voltages required to observe a remarkable change in the magnetic properties of cobalt oxide were rather large, of the order of −50 V. Recently, we showed that magneto-ionics depends on the electrical properties of the target materials.4 Here we demonstrate that not only the electrical properties of cobalt oxide are important, but also the composition of the electrolyte. More specifically, its ionic strength also plays a key role in magneto-ionics. In the past years, various salts and additives have been added to solvents to increase the ionic strength of electrolytes for a variety of purposes.17–19 As the salt concentration is increased, more ions can accumulate in the compact layer of the EDL, reducing the presence of free solvent molecules in the vicinity of the electrode. As a result, the performance of energy storage systems improves.17,20 This strategy could well work for magneto-ionics, paving the way for higher charge accumulation at the surface of the solid material and, hence, more intense electric fields. To date, different electrolytes have been tested for voltage-driven ion migration and, in some cases, salts were added to the solvent (e.g. LiPF6 in dimethyl carbonate/ethylene carbonate mixture) to observe the effects.7,21,22 In spite of the intensive research carried out in the last decade, studies with complex PC formulations are lacking.
Herein, we have investigated the impact of the addition of inorganic salts, namely potassium iodide (KI), potassium chloride (KCl) and calcium tetrafluoroborate (Ca(BF4)2), to anhydrous PC on the magneto-ionic effects induced in 15 nm-thick Co oxide films. The solubility of KI and KCl in PC at room temperature was reported by Peruzzi et al.23 and that of Ca(BF4)2 in PC was investigated by Forero-Saboya et al.17 (see Experimental section). KCl was primarily chosen as it is the electrolyte support of choice in many electrochemical processes taking place in aqueous solutions. KI was selected as it showed higher solubility in PC and simply implied the replacement of Cl− by I−. Finally, Ca(BF4)2 was chosen since it is typically dissolved in alkyl carbonates like PC in calcium ion batteries.24 Our work reveals that improvements in oxygen ion motion25–27 in cobalt oxide are accomplished by adding these salts to PC. Specifically, the fastest magneto-ionic rate is observed when using PC + 2.5 × 10−4 M KI electrolyte, which is 35 times larger than the rate observed for bare PC electrolyte under −1.5 V. Moreover, upon biasing Co oxide for one hour, the same PC + 2.5 × 10−4 M KI electrolyte results in the largest generation of magnetization. The process is highly reversible for all added salts since the generated magnetism can be reduced after applying a voltage of opposite polarity (i.e., +1.5 V). The magneto-ionic response of the cobalt oxide films was further studied at varying concentrations of KI dissolved in PC. Our results show that improved magneto-ionics can be achieved by conveniently tuning the EDL strength via liquid electrolyte engineering.
The magnetic moment of cobalt oxide in different electrolyte solutions was measured at room temperature under a 10 kOe magnetic field, where the generated ferromagnetic response is saturated. The external voltage was applied in situ during the magnetic measurements. Fig. 1(d) presents the time evolution of magnetization change (ΔM − t) for the films actuated in bare PC and PC containing 2.5 × 10−5 M KI, KCl and Ca(BF4)2 electrolytes. In the first stage of the measurements, ΔM continuously increases to around 30 emu cm−3 for the bare PC electrolyte while ΔV = −1.5 V is applied for 60 min (i.e., t = 65 min) (see the green shaded region in Fig. 1(d)). This indicates the appearance of ferromagnetism in the cobalt oxide. In the second stage (i.e., after applying +1.5 V for 25 min), ΔM sharply drops due to the reversal of the bias polarity, and reaches around 10 emu cm−3. The occurrence of a ferromagnetic-paramagnetic (ON–OFF) transition in the oxide films is related to voltage-induced oxygen ion motion.10 Several observations can be made from the ΔM − t curves for electrolytes with different inorganic salts. First, for the PC + KCl electrolyte, ΔM increases at a similar rate as the bare PC one until t = 20 min, and it then grows faster and approaches 40 emu cm−3 at t = 65 min, representing a 33% increase compared to bare PC. Importantly, the initial ΔM change is significantly enhanced with the additions of KI and Ca(BF4)2 into PC, as reflected by the larger slopes of the blue and red curves for t < 20 min and t < 35 min, respectively. Furthermore, the maximum ΔM values at t = 65 min are much higher in the electrolytes containing KI and Ca(BF4)2 than for bare PC and PC + KCl. Remarkably, the maximum ΔM for PC + 2.5 × 10−5 M KI electrolyte is twice higher than that for bare PC (70 emu cm−3versus 30 emu cm−3). Finally, the sudden decrease of ΔM when applying voltage of opposite polarity is observed for all the electrolytes. In particular, ΔM drops from around 70 emu cm−3 to 10 emu cm−3 during the time interval from t = 65 min to 70 min for the electrolyte made of PC + 2.5 × 10−5 M KI. These observations indicate that magneto-ionic effects in cobalt oxide can be substantially improved by electrolyte engineering. It is worth mentioning that the relatively small gating voltage employed in the current study (1.5 V) can produce similar magneto-ionic responses as previous works where we used applied voltages of the order of 25 V or higher for similar Co oxide film thicknesses.11,12 This decrease in the threshold voltage needed to induce changes in the magnetic properties of the Co oxide can be directly linked to the addition of inorganic salts into PC. Interestingly, although one would expect KCl and KI to yield similar results upon negatively biasing the cobalt oxide film, ΔM was far higher for KI.
To get atomistic insights on the initial cobalt oxide – propylene carbonate + KX (X = Cl, I) interface, ab initio molecular dynamics (AIMD) simulations at 300 K were carried out. Co3O4 was considered for the simulations. Energies were computed at the PBE-D3+U (Ueff = 3.0 eV) without applying any external potential. The statistical analysis was performed on the last 8 (6 depending on the structure) ps of each simulation (see Computational details). We paid attention on the location of KX (X = Cl or I) and thus, two different initial structures were considered for each salt (Fig. S1 of the ESI†). In one case, the two ions were directly interacting with the surface at distances around 2 Å (KXAds). In the other, the salt was fully solvated by PC molecules (KXSol). Fig. 2 reports: (a) one representative snapshot of the simulation leading to the most favorable conformation for each salt KClAds and KISol AIMD, (b) the variation of the surface–ion distances in the simulations leading to the most favorable situation and (c) the energetics of the four AIMD. The variation of the potassium–surface distance, the anion–surface distance and a representative snapshot of the four simulations can be found in Fig. S2, S3 and S4 of the ESI.†
The AIMD simulations starting with the two ions adsorbed on the surface evolved without any relevant variation. All ions remain attached at the surface with average ion···surface distances of 2.2, 2.1 and 2.4 Å for K+, Cl− and I−, respectively. In these simulations no significant charge separation is generated, suggesting that almost no positive charge will be accumulated on the Co3O4 surface. The simulations starting with the two ions in the solution (KClSol and KISol) showed a larger reorganization. Regardless of the counter ion, K+ rapidly becomes adsorbed on the surface with K···surface average distances that are only slightly higher than in the KXAds simulation (2.5–2.6 Å). In contrast, the anions remain in the solution. The Cl− anion moves around the initial structure with an average surface–Cl− distance of 6.5 Å. Iodide prefers to move further away from the surface, the resulting surface–anion distances becoming about 9.8 Å. That is, the KXSol simulations lead to a structure defining an EDL, with a compact positive charge accumulation on Co3O4. Comparison between the energetics of the KXAds and KXSol simulations rises the different behavior of the anions. For KCl, the configuration in which the two ions are directly adsorbed on the surface is slightly more stable (ΔG = 0.2 eV) than the structure defining the double layer. In contrast, for KI, there is a large preference (ΔG = −1.0 eV) for the conformation that accumulates positive charge on the surface. This can be attributed to the largest ionic radius of I− when compared to Cl− that makes all electrostatic interactions (and particularly that with the surface) weaker. While the AIMD simulations are carried out without applying an external potential, one can expect that upon externally biasing Co3O4 layer with negative voltages, the structure accumulating positive charge on the surface would be favored with respect to that with the two ions close to the surface but without modifying the trends between the two ions. Consequently, simulations shows that KI favors the structure accumulating more positive charge over Co3O4 and, in turn, generates a stronger electric field.
In order to further optimize the magneto-ionic response for the KI-containing PC electrolyte, the room temperature magnetic moment as a function of biasing time were recorded with a 10 kOe field and varying KI concentrations (from 2.5 × 10−6 M to 2.5 × 10−3 M). Upon biasing for 1 hour, the ΔM first increases as the KI concentration increases from 2.5 × 10−6 M to 2.5 × 10−4 M, and then it decreases with further addition of KI. At 2.5 × 10−3 M KI, the oxide film peeled off, possibly because of the strong electrochemical reactions taking place (see the dashed curve in Fig. 3(a)). Indeed, the solution acquired a yellow color, indicating the formation of I2 gas at the Pt counter electrode, and the subsequent formation of I3− according to the reaction:
I2(g) + I(aq)− = I(aq)3− | (1) |
Remarkably, after applying −1.5 V for 1 hour, the maximum ΔM for 2.5 × 10−4 M KI electrolyte (≈280 emu cm−3) is more than one order of magnitude larger than that for bare PC (≈25 emu cm−3). The achieved magneto-ionic rate (i.e., the rate at which the ferromagnetic signal from metallic Co is generated) is drastically enhanced from 5 emu cm−3 min−1 for bare PC to 184 emu cm−3 min−1 for PC + 2.5 × 10−4 M KI (see Fig. 3(b)). Moreover, partial recovery under an opposite bias of +1.5 V was observed for the best performing KI concentrations of 2.5 × 10−4 M and 2.5 × 10−5 M (Fig. 3(c)). Room temperature hysteresis loops of the voltage-actuated cobalt oxide films confirm the effect of the KI concentration in PC on the ON–OFF ferromagnetic switching for this system (Fig. 4). This corroborates that magneto-ionic effects have a strong dependence on the KI concentration.
To gain information on the chemical environment of the cobalt oxide film surface, XPS analyses were carried out before and after ME experiments. The Co 2p core-level XPS spectra of as-prepared sample, and samples treated using bare PC and PC + 2.5 × 10−4 M KI are shown in Fig. 5. For the as-prepared sample (see Fig. 5(a)), the two major peaks at 780.1 eV and 795.9 eV match Co 2p3/2 and Co 2p1/2 binding energies, respectively, of CoO and/or Co3O4 phases.12,28,29 The satellite structure at higher binding energies can be ascribed to the shake-up process of the Co2+ species in the high-spin state. Aside from these four peaks, Fig. 5(b) clearly shows two shoulders (indicated by the downward arrows) on the lower binding energy side of the major peaks for bare PC-treated sample. The best fitting of the spectrum results in two additional XPS peaks located at 778.3 eV and 793.3 eV, which are the characteristic binding energies of Co 2p3/2 and Co 2p1/2, respectively, for metallic Co.2 This unambiguously confirms the reduction of cobalt oxides into Co upon negative voltage actuation in bare PC electrolyte. Interestingly, the relative intensities of these additional peaks and, importantly, at the expense of the oxide Co 2p peaks, become dominant in the case of the film electrolyte-gated in PC + 2.5 × 10−4 M KI. This indicates the formation of significant amounts of metallic Co and, accordingly, higher ΔM as seen in ME experiments. Moreover, it is instructive to point out that there are no observable traces of iodine in the survey spectrum on PC + 2.5 × 10−4 M KI-treated sample (not shown), ruling out the possibility of formation of magnetic iodine-containing compounds. Overall, the formation of metallic Co upon voltage application can be written as:
CoO → Co + VÖ | (2) |
Co3O4 → 3Co + 4VÖ | (3) |
To further examine the reversibility of the magneto-ionic effects of the cobalt oxide film in the PC +2.5 × 10−4 M KI electrolyte, voltage pulses of −1.35 V and +1.35 V (of 10 min each) were alternated, and clear changes are observed in ΔM running in parallel to voltage actuation (Fig. 6). Note that up to 5 magneto-ionic cycles could be obtained with these applied voltage pulses.
The Co3O4-propylene interface was represented with a 4-layers thick slab model of the (110) facet where 13 propylene carbonate molecules were added in the vacuum space between images to reproduce the solvent density at room temperature (r = 1.2 g cm−3). Furthermore, a KX (X = Cl or I) unit was included to represent the dissolved salt. Two initial starting configurations were considered for each salt (Fig. S2, ESI†): (a) the two ions are initially located on the surface, directly interacting with Co3O4, and (b) the ions are solvated by propylene carbonate molecules and thus located at about 6 Å from the surface. Further details can be found in the supporting information.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2nh00340f |
This journal is © The Royal Society of Chemistry 2023 |