Open Access Article
Samantha
Phan†
a,
Jonathan J.
Ramtahal†
b and
Christine K.
Luscombe†
*c
aDepartment of Chemistry, University of Washington, Seattle, WA 98195, USA
bShimoda Marine Research Center, University of Tsukuba, Shimoda 5-10-1, Shizuoka, 415-0025, Japan
cDepartment of Materials Science and Engineering, University of Washington, Seattle, WA 98195, USA
First published on 8th April 2026
The use of spectroscopic techniques to identify microplastics found in the environment is challenging because weathered microplastics undergo chemical changes that make their spectra drastically different from their pristine counterparts. In previous work, we reported the findings from systematic artificial weathering of polyethylene and polypropylene for 0–26 weeks in four different weathering environments (air, DI water, artificial seawater, and Puget Sound seawater), characterized by Raman and IR spectroscopy (https://doi.org/10.1016/j.polymertesting.2022.107752). This manuscript provides the final part of the study's findings, which includes the Raman and IR spectroscopy information on the weathering effects on polystyrene (PS), polyethylene terephthalate (PET), and nylon 6 (PA6) with the goal to evaluate how these weathering effects affect the reliability of polymer identification. Our results show that spectral changes are often non-linear, lacking a clear exposure-time trend. While PS exhibited significant oxidation by IR in DI water, these changes were not detectable by Raman spectroscopy, highlighting a risk for researchers who rely on a single technique. Both PS and PA6 showed more degradation peaks in DI water than in seawater, which suggests that chlorine radicals from salt may inhibit the formation of some degradation products. This work underscores the need to use complementary IR and Raman analysis to avoid misinterpretation of environmental microplastics and their aging state.
Environmental weathering of microplastics is a complex process and is influenced by climate, regional conditions, and many other factors that are difficult to control in the laboratory.11 The major processes involved in plastic degradation can differ depending on the conditions in which plastics are found and must be understood to assess potential hazards.11,12 Microplastic degradation can be owed to both mechanical and chemical processes which can be summarized as follows: (1) photodegradation – the action of light, (2) thermooxidation – slow oxidative breakdown at moderate temperatures, (3) thermal degradation – action at high temperatures (industrial or environmental), (4) hydrolysis – reaction with water, and (5) biodegradation – the action of organisms (i.e., microbes).13 In the natural environment, these different processes of degradation act in collaboration and in interaction with each other, with photodegradation as the main process.13 Depending on the functional groups present in a polymer, this can lead to a myriad of reactions and processes that result in many different chemical changes and byproducts.
The accurate identification of environmental microplastics remains a major methodological challenge mainly because of the diversity of polymers coupled with the various physicochemical changes as a result of environmental weathering. Many studies rely on visual identification and sorting microplastics from non-plastic materials. Although rapid and cost-effective, these methods often introduce misidentification, leading to systematic over or under estimation of microplastic concentration. Spectroscopic techniques including Raman microspectroscopy (µ-Raman) and Fourier transform infrared microspectroscopy (µ-FTIR) are robust non-destructive methods that can be employed for polymer confirmation. While more reliable than visual identification, a major limitation of these methods lies in the availability and quality of comprehensive spectral libraries.4,5,13–16 Environmentally weathered microplastics often exhibit altered functional groups, surface oxidation, and physical degradation relative to pristine polymers. Such alterations greatly reduce spectral matching reliability. This is further complicated when attempting to separate microplastics from their environmental matrices and measurement of significantly weathered microplastic surfaces.17,18 Researchers are working to incorporate weathered spectra into libraries,4,5,8,9 but this is complicated by the fact that environmental degradation is far more complex than laboratory simulations can effectively replicate.
Previously, we began to address this lab-to-environment gap by studying polyethylene (PE) and polypropylene (PP).15 We found that they show variations in crystallinity and oxidative byproducts depending on the weathering condition (air, DI water, artificial seawater, and Puget Sound seawater), with samples in Puget Sound seawater showing the greatest changes. However, polyolefins such as PE and PP are not the only polymers commonly found in the environment. To expand the understanding of the effect of varying weathering conditions on IR and Raman spectral changes to other common polymer types, here, we present the remaining weathering results of polystyrene (PS), polyethylene terephthalate (PET), and nylon 6 (PA6) and elaborate on the complexities of their spectral changes.
000 and a density of 1.06 g mL−1. PET pellets were about 4 mm in size and had a density of 1.68 g mL−1. PA6 pellets were about 3 mm in size and had a density of 1.084 g mL−1. The Mw value of PS was provided by Sigma-Aldrich, but values for PET and PA6 pellets were not reported. Sea salts (NutriSelect® Basic) were purchased from Sigma-Aldrich as an artificial seawater mix. Water, collected directly from the surface of the Puget Sound (47.616844, 122.358928) in a glass container without any filtration or treatment, was also used for the studies within 24 h of collection.
The light source for solar irradiation was Tungsten halogen Solux 4700 K light bulbs, which were chosen to match the AM1.5 solar spectrum at 25 °C.23,24 The 4700 K tungsten halogen Solux lamps were used by Reese et al. to test photoinduced degradation of polymer and polymer–fullerene active layers in photovoltaics, and comparative data of the lamp used for illumination conditions relative to AM1.5G are available in the SI (Fig. S1).23 Subsequently, Holliday and Luscombe used the same lamp to investigate photooxidative stability in organic photovoltaics.24 On clear, cloudless days, the solar irradiation is 1000 W m−2; however, this value is greatly influenced by angle, organisms, water vapor, suspended particles, etc.15 The lightbulbs were positioned as in the study of Phan et al., 11 cm from the edge of the top tray and 16 cm above the top of the tray.15 The lightbulbs were connected to a lightbulb socket, a transistor, and a mechanical timer that allowed 12 h of continuous light irradiation and 12 h without irradiation to mimic a typical day. The radiance on the vials ranged from 85 to 159 W m−2, depending on the vial location, which was measured with a Topcon spectroradiometer. The vials were regularly rotated and monitored to ensure that all samples received the same average light exposure and that the temperatures remained at 25–30 °C over the 26 weeks. The glass vials were sufficient to allow all wavelengths of light to pass. One aliquot pellet of each sample was taken out every 2 weeks for 10 weeks and then at 26 weeks of irradiation to observe any long-term changes. Each aliquot was rinsed with copious amounts of DI water (especially for samples exposed to salt water), placed in a vial, and dried in a desiccator at room temperature before characterization. Spectra were taken on multiple points on any given pellet to provide statistically meaningful data.
Our results contrast with previous studies33 in which Raman peak changes in PS, exposed to natural sunlight at higher temperatures (35.8–37.4 °C), were observed. This discrepancy likely highlights the influence of experimental conditions, as elevated temperatures and different irradiance levels can lead to different chemical reactions during degradation.34–37 Another difference was the instrumentation: our study used a 785 nm laser, while Kilinc et al. used a 532 nm laser.33 Chemical modification can occur to varying degrees on the surface and in the bulk. We hypothesized that our laser's deeper penetration (12 µm for 785 nm vs. 0.7 µm for 532 nm)38,39 might obscure surface changes. However, our additional characterizations with a 532 nm laser source still revealed no significant differences (Fig. S6), confirming our initial finding.
In the context of the Puget Sound, where one of the water samples for weathering was taken, this region receives significant cloud coverage throughout the year, which decreases the solar irradiance and slows environmental photodegradation.40 The irradiance in Kilinc et al.'s33 study ranged between 791 W m−2 and 890 W m−2, which is 6–9 times higher than the irradiance in this study. It is likely that the level of light exposure to the PS samples in this study, though similar to the environment of the Puget Sound, is insufficient to induce any observable changes to the Raman spectra. This is particularly interesting because Raman measurements of PS extracted from marine organisms,4,5 from the Puget Sound, also showed that the Raman spectra of PS were similar to reference spectra of PS with few appearances and no disappearances of characteristic Raman spectral peaks, while other polymers, such as PP, nylon, and PET, show more spectral variances. This demonstrates the importance of investigating different weathering conditions on the chemical changes of microplastics to ensure adequate plastic identification.
In contrast to Raman, IR spectroscopy revealed the various peaks associated with oxidative functional groups, such as OH, C–O, and C
O groups, when PS was subjected to increasing light exposure and appeared in all the different weathering conditions (Fig. 1). In weathered PS, the formation of a band around 3464 cm−1 and an intensity increase at 1745 cm−1 indicated the formation of hydroperoxy and carbonyl groups, respectively.41 The phenyl ring in PS can be excited and, through intersystem crossing, form a triplet state under UV radiation.12 That triplet energy can be transferred to nearby C–H or Ph–C bonds.11,12,14 The cleavage of those bonds can form polystyryl radicals, which are converted to peroxy radicals that participate in crosslinking and chain scission, resulting in the formation of ketones, styrene monomers, and olefins.11,14
In contrast to the single new peak at 1410 cm−1 in the air-weathered IR spectra, samples weathered in water showed broad bands around 3350 cm−1 and between 1745 cm−1 and 826 cm−1. These findings suggest the formation of diverse, oxidized species for the water samples (Table 1 and Fig. 1). All water conditions showed hydroxyperoxide formation (bands 3390–3232 cm−1), supported by peaks around 1300 cm−1.15,41 Hydroxyperoxides, also seen in weathered PP, act as major sources of free radicals during photodegradation.15,42
| Peak position (cm−1) | Vibrational mode | Weathering condition | |||
|---|---|---|---|---|---|
| Air | DI | AS | PSS | ||
| DI = deionized water, AS = artificial seawater, PSS = Puget Sound seawater.a Indicates peak changes. | |||||
| 3520, 3464, 3400, 3347, 3220a | R–O–OH15,57 | × | × | × | |
| 3550–3220a | O–H stretch41,57 | × | × | × | |
| 3084, 3060, 3025 | Aromatic CH stretch46,58,59 | × | × | × | × |
| 2920, 2850 | CH2 asymmetric and symmetric stretch46,58 | × | × | × | × |
| 1745,a 1730a | C O stretch41 |
× | × | × | |
| 1664a | C C stretch47 |
× | |||
| 1640a | C C or C O43 |
× | × | × | |
| 1601, 1493, 1452 | Aromatic ring modes46,58,59 | × | × | × | × |
| 1344a | Unknown | × | |||
| 1280,a 1242a | C–O stretch41 | × | |||
| 1115a | Aromatic skeleton and C–O stretch60,61 | × | × | × | |
| 1080a | C–O, phthalate, secondary alcohol41,46 | × | |||
| 857a | C–H wag, para-substituted aromatic46 | × | |||
| 826a | C–H wag, meta-substituted aromatic46 | × | |||
| 758 | Aromatic out-of-plane CH bend58 | × | × | × | × |
Upon closer examination of the IR spectra of PS samples weathered in water, PS weathered in DI water exhibited the most unique peaks (1664, 1547, 1372, 1344, 1280, 1242, and 826 cm−1) compared to PS weathered in the other water conditions. This suggests that PS weathered in DI water may differ from other the weathering conditions resulting in the production of C
O, O–O, and C–O bond-containing byproducts. Though beyond the scope of this study, an in-depth mechanism analysis regarding the effects of water molecules on the free radical reaction pathways of PS degradation will be useful in elucidating the origin of the oxidative peaks in DI water. The IR spectrum of PS weathered for 10 weeks in Puget Sound seawater appears similar to pristine PS. This could indicate some flaking of the PS surface, similar to PE,15,43 as weathered PS also showed surface cracking (Fig. 2). Another explanation is that salinity has a greater influence on the weathering for PS, as the functional group formation for PS weathered in artificial seawater and Puget Sound seawater is similar, but different for PS weathered in DI water.
In seawater, NaCl contributes to about 90% of its salinity concentration.44 The Cl− in seawater can inhibit the photoaging of microplastics because reactive chlorine radicals
could quench perhydroxyl radicals
.45 With perhydroxyl radicals quenched, the free radical chain reaction under light irradiation would be inhibited, which explains the fewer unique peaks in PS weathered in the seawater conditions. In DI-water weathered PS, various C
C bonds were observed (Table 1), which indicates that chain scission resulted in the formation of different olefins. The intensity changes in the peaks around 3400 cm−1 and 1640 cm−1 in PS weathered in the water conditions were much greater than those observed in PS weathered in air. Unique to PS weathered in the Puget Sound seawater was the formation of a peak at 1080 cm−1, which indicates a C–O stretch from a secondary alcohol.41,46 The formation of more unique IR peaks for DI water-weathered PS compared to the Puget Sound seawater-weathered PS is a notable difference from previous findings for weathered PP, where PP weathered in Puget Sound seawater showed more peaks associated with C–O–C and O–O stretches between 1300 and 900 cm−1.15 PP weathered in Puget Sound seawater also exhibited the formation of unique hydroperoxides compared to the other weathering conditions, along with groups indicative of crosslinking and chain scission that resulted in increased crystallinity in the weathered samples.
While the contradictory results for PP and PS may be due to their different chemical structures, another possibility is the role of microbial action. PS is known to release toxic aromatic VOCs during degradation, which could inhibit microbial activity.47–49 In contrast, the byproducts of PP may be less toxic, potentially allowing for microbial degradation to occur. This study did not analyze VOCs or microbial composition, so this remains a hypothesis that warrants future investigation.
The degree of weathering can be monitored by the carbonyl index (CI),50 the ratio of the carbonyl band and the reference band, which, in the case of PS, is the CH2 stretching band.51,52 The CI for PS can be calculated by eqn (1):
![]() | (1) |
C bonds indicates the cleavage of the polymer chain.53 The degradation of PS has been reported to occur in two stages, where Stage I is dominated by photooxidation in the near-surface layer, followed by Stage II, where microcrack formation and particle rupture accelerate degradation.54 As such, the fluctuation of the CI may be due to the repeated photooxidation and then cracking or flaking of the PS surface, which then results in the exposure of less weathered PS (Fig. 2).55,56
These findings for PS highlight a methodological challenge. While Raman spectroscopy was unaffected by weathering, similar to our findings for PE and PP, it failed to detect the significant oxidation that occurred. Conversely, IR spectroscopy did detect this oxidation, but in severe cases, these new weathering bands obstructed polymer identification. For example, PS weathered for 26 weeks in Puget Sound seawater showed strong weathering bands (around 3250, 1640, and 1100 cm−1) that obscured the polymer's identifying IR peaks. Artificial seawater samples showed similar, albeit less intense, bands. This presents a challenge for single-method analyses: Raman may falsely identify the plastic as pristine, while IR may fail to identify the polymer at all. These results emphasize that relying on one technique can lead to false negatives and underestimation of microplastic pollution.
| Peak position (cm−1) | Vibrational mode | Phase or associated features |
|---|---|---|
| 3083, 3068, 3000 | Ring C–H stretch (benzene ring)64,65 | Orientation of species perpendicular to the polymer chain |
| 2964 | –CH2– groups adjacent to O atoms64,65 | — |
| 1725 | C O stretch29,64,65,67 |
Crystalline |
| 1615 | C–C/C C symmetric stretch (1,4 carbons in benzene ring)29,64,65,67 |
Orientation of the polymer backbone chain |
| 1451 | CH2 and OCH bending65 | — |
| 1413 | CCH bending and OCH bending65 | — |
| 1370 | CH2 wag/bend64 | — |
| 1352 | Ring breathing modes of sp2 carbon63 | — |
| 1285 | C–C ring stretch, C–O stretching64,65 | — |
| 1179 | Ring C–H in plane bend, C–C stretch64,65 | — |
| 1120 | Ring C–H in-plane bend, ester C(O)–O, gauche ethylene glycol C–C stretch29,64 | — |
| 1105, 1129 | Ester C(O)–O, ethylene glycol C–C stretching69 | — |
| 1097 | C–O, C–C stretch, ring C–C, ester C(O)–O, trans ethylene glycol C–C stretching29 | Crystalline |
| 890 | CH2 rocking64 | — |
| 860 | C–C, C–O–C bend, ring C–C breathing (Ag mode), ester C(O)–O stretch29 | — |
| 853 | C−C stretch (ring breathing), C−O stretch64 | — |
| 797 | Ring C–H out-of-plane bend64 | — |
| 632 | Ring CCC in plane bend64 | — |
One common method to track PET crystallinity with Raman is to analyze the ratio between the 1097 cm−1 and 1120 cm−1 peaks, which correspond to the trans (crystalline) and gauche (amorphous) conformations of the ethylene glycol unit, respectively.29,64,65 However, when we applied this analysis, our PET samples showed peak differences in this region, and the results were inconclusive. This may be due to water acting as a plasticizer, promoting chemi-crystallization in the amorphous regions.66
We therefore turned to another peak long associated with crystallinity: the C
O stretch at 1725 cm−1.67,68 We found that all weathering conditions exhibited fluctuations in this stretch, with Puget Sound seawater and artificial seawater weathering showing significantly more variability (Fig. 3 and Fig. S9). While higher crystallinity is known to narrow this peak, our samples in water conditions had similar peak widths to those weathered in air (Fig. S9). This suggests that the greater intensity variation in artificial seawater and Puget Sound seawater indicates a change in the C
O stretching moieties rather than a change in crystallinity.
Finally, we examined the 1615 cm−1 peak, where a decrease indicates more aligned benzene rings.29,67 We observed minimal variations in air, DI, and artificial seawater, but slightly more variation in Puget Sound seawater. Taken together, these findings suggest that saltwater weathering (artificial seawater and Puget Sound seawater) alters C
O moieties and polymer backbone orientation, while Puget Sound seawater also increases structural disorder (as supported by the sp2 carbon ring fluctuations).
IR spectroscopy is more sensitive to polar functional groups than Raman spectroscopy and is well-suited to elucidate oxidative functional groups formed during weathering. However, the IR spectra of PET weathered in all the conditions showed few peak changes and no disappearances of characteristic identification peaks (Fig. 4 and Table 3); this is a stark difference from weathered PE, PP, and PS, where IR spectroscopy revealed more weathering effects than Raman spectroscopy. Weathered PET exhibited a peak at approximately 3300 cm−1, indicating the formation of OH groups, with more intense peaks observed in artificial seawater and Puget Sound seawater. The higher formation of OH groups in simulated marine weathering is consistent with other studies,43,74 as hydrolysis is the primary degradation process of PET and results in carboxyl or hydroxyl-terminated end groups in the polymer chains.74
| Peak position (cm−1) | Vibrational mode | Weathering condition | |||
|---|---|---|---|---|---|
| Air | DI | AS | PSS | ||
| DI = deionized water, AS = artificial seawater, PSS = Puget Sound seawater.a Indicates peak changes. | |||||
| 3550–3220a | O–H stretch57 | × | × | × | × |
| 2962, 2920,a 2895, 2852a | Aliphatic C–H stretch, CH2 stretch70,71 | × | |||
| 1714 | C O stretch, aromatic ester72 |
× | × | × | × |
| 1685 | C O (CO, CO2, –COOH end group)72 |
× | × | × | × |
| 1645a | –COOH72 | × | × | ||
| 1577, 1504 | C C ring stretch, C–H ring in-plane bend70,71 |
× | × | × | × |
| 1470a | CH2 bend, trans71 | × | × | ||
| 1455 | CH2 bend, O–CH bend70 | × | × | × | × |
| 1409 | Phenylene in-plane ring deformation70,72 | × | × | × | × |
| 1370, 1340 | CH2 wag cis, CH2 wag trans70,71 | × | × | × | × |
| 1266 | C–O stretch carbonyl, C–C ring ester stretch, C O in plane bend71 |
× | × | × | × |
| 1172 | C–H ring in-plane bend, C C ring stretch71 |
× | × | × | × |
| 1100 | C–O–C stretch, asymmetric methylene group stretch70,73 | × | × | × | × |
| 944a | Unknown | × | |||
| 873 | C–H ring out-of-plane bend, C–C ring ester out-of-plane bend, C O out-of-plane bend, ring torsion71 |
× | × | × | × |
| 815–854,a 918a | Unknown | × | × | × | |
| 725 | C–H ring out-of-plane bend, –C O out-of-plane bend70,71 |
× | × | × | × |
Uniquely, PET weathered in Puget Sound seawater showed increased IR intensity at 2920 cm−1 and 2852 cm−1 (C–H bending/stretching),70,71 which was not observed in other weathering conditions. While requiring further investigation, this could potentially arise from the breakdown of phosphite antioxidants commonly used in PET (unlike phenolic antioxidants, which cause discoloration).75 Indeed, characteristic peaks for such additives (e.g., C–H stretches ∼2900 cm−1, –SO3− ∼1242 cm−1) are visible in our spectra (Fig. 4). The presence of these stabilizers might also explain the relatively minor IR spectral changes observed for PET overall compared to PS.
In contrast to PE, PP, and PS, the quantification of carbonyl content as a result of the weathering of PET is not as straightforward because of the inherent presence of the ester C
O stretch at 1714 cm−1.76 A combination of factors is associated with the intensity of the 1714 cm−1 peak; a decrease in absorbance intensity indicates ester bond scission, while an increase indicates the formation of carbonyl-containing degradation products. When normalized to the phenylene ring vibrational reference peak at 1410 cm−1, which is independent of polarization and sample orientation,72,77 the absorbance intensity of the 1714 cm−1 peak slightly decreases over time in all weathering conditions (Fig. S10). Puget Sound seawater-weathered PET also shows a decrease in the 1714 cm−1 intensity from 0 to 10 weeks, but at 26 weeks, the CI is similar to pristine PET, which may indicate flaking of weathered PET over time.
In more detail, the aromatic-containing main chain of PET absorbs UV radiation during photodegradation, inducing chain scission of the ester bonds in the backbone and leading to a decrease in molecular weight and oxidation. This process proceeds through Norrish type I (which involves radical formation and cleavage of the α C–C bond adjacent to the carbonyl) and II (which involves intramolecular hydrogen abstraction from a γ carbon to a carbonyl oxygen) reactions to form carbonyl and carboxyl-containing products.66,72,74,78
To assess weathering by accounting for both ester bond scission and the formation of new carboxylic acid groups, the CI for PET is calculated from the ratio of the degradation product peak at 1685 cm−1 to the original ester peak at 1714 cm−1, as shown in eqn (2):72,79,80
![]() | (2) |
Spectral deconvolution resolved the overlapping absorbance in the carbonyl region to distinguish the ester and carboxylic groups. With increasing light exposure, the CI slightly increased in the air weathering condition and the CI decreased in the water weathering conditions (Fig. S11). Water promotes the hydrolysis of PET, and it is unsurprising that when weathered in water, it undergoes ester bond cleavage more readily than when weathered in air. The results also indicate the accumulation of oxidative degradation products in air-weathered PET. For PET weathered in artificial seawater and air, after 26 weeks, the CI was comparable to pristine samples. This may be an indication of flaking of the plastic surface to expose new, less weathered surfaces, followed by further degradation. In some cases, PET weathered in artificial seawater and Puget Sound seawater produced large peaks at 1645 cm−1, indicative of acid-terminated hydrolysis products72 that obscured the 1685 cm−1 peak completely and made it challenging to accurately determine the CI.
O stretch) (Fig. 5 and Table 4). Notably, we found that PA6 weathered in water conditions exhibited more variation in these peaks than samples weathered in air. These variations indicate changes to the polymer backbone, likely due to oxygenated radicals reacting with the C–N peptide bond to initiate chain scission and form new carbonyl groups.83,84
| Peak position (cm−1) | Vibrational mode | Phase or associated features |
|---|---|---|
| 2930 | C–H stretch85 | — |
| 1637 | C O stretch85–87 |
Amide I |
| 1467, 1480 | C–N stretch, N–H bend30,86,88 | Amide II, α-phase |
| 1444 | CH2 bend85,86 | — |
| 1370 | CH2 wag86 | — |
| 1305 | CH2 twist85,89 | β-phase |
| 1280 | C–N stretch, N–H bend85,86 | Amide III |
| 1126 | C–C stretch30 | Brill transition |
| 1081 (main), 1060, 1121 | C–C stretch86–89 | All-gauche CC backbone, γ-phase |
| 1062, 1080, 1127 | C–C stretch86,88,89 | Mesomorphic, β-phase |
| 1063, 1075, 1129 | C–C stretch85,86 | All-trans CC backbone, α-phase |
| 932 | C–CO stretch, CO–NH in plane85,88,89 | α-Phase |
| 925 | CO–NH in plane89 | γ-Phase |
| 833 | CH2 rock90 | α-Phase |
As an initial examination, the 1637 cm−1 peak (amide I C
O stretch) was monitored to calculate a Raman CI (Fig. S12). The analysis showed that samples weathered in air, artificial seawater, and Puget Sound seawater exhibited an increase in this peak, followed by a decrease, with 26 week samples showing similar levels to pristine PA6. Samples in DI water, however, showed no specific trend. This lack of a clear trend corroborates findings by Fernández-González et al., who also found that weathered PA6 spectral bands showed no trend over time.82
To further probe changes in PA6's complex crystalline structure at the surface, we tracked the intensity ratio of the 1081 cm−1 (associated with the γ-phase) and 1062 cm−1 (associated with all phases) peaks as a first-order approximation (Fig. S13). This ratio increased over time in air and Puget Sound seawater but decreased over time in DI and AS. This suggests that when PA6 is weathered in air and Puget Sound seawater, the percentage of the γ-phase increases, implying the C–C sections of the backbone adopt more gauche configurations.
When examining weathered PA6 using IR, most identifying peaks were still present across the weathering conditions, although in some samples, weathering bands attributed to OH and C–O formation did develop. PA6 weathered in air showed very few formations of new IR spectral peaks, while samples in DI water showed more unique peaks not found in the other weathering conditions from 1417 cm−1 to 726 cm−1 (Fig. 6). Puget Sound seawater weathered samples showed the formation of bands around 3335 cm−1 (OH stretch), 1732 cm−1 (C
O stretch), and 1106 cm−1 (Table 5). All weathering conditions resulted in PA6 exhibiting a slight decrease in the 3081 cm−1 peak, which is assigned to the N–H deformation and C–N stretch.
| Peak position (cm−1) | Vibrational mode | Weathering condition | |||
|---|---|---|---|---|---|
| Air | DI | AS | PSS | ||
| DI = deionized water, AS = artificial seawater, PSS = Puget Sound seawater.a Indicates peak changes. | |||||
| 3550–3220a | O–H stretch57 | × | × | × | |
| 3295 | N–H stretch, amide II91,92 | × | × | × | × |
| 3081a | N–H stretch92 | × | × | × | × |
| 2933 | Symmetric CH2 stretch91,92 | × | × | × | × |
| 2860 | Asymmetric CH2 stretch91,92 | × | × | × | × |
| 1732 | C O stretch, imides83,93 |
× | × | × | × |
| 1635 | C C stretch, amide 191,93 |
× | × | × | × |
| 1540 | N–H bend, amide II91,93 | × | × | × | × |
| 1417a | CH2 scissor92 | × | |||
| 1372 | CH2 wag, amide III92 | × | × | × | × |
| 1261 | N–H bend, C–N stretch92 | × | × | × | × |
| 1201a | CH2 twist-wag, α-phase92 | × | × | × | × |
| 1169 | CO–NH skelal90 | × | × | × | × |
| 1080a | Unknown, γ-phase90 | × | × | ||
| 1073 | C–C stretch90 | × | × | × | × |
| 959, 950, 929 | CO–NH in plane, α-phase90,92 | × | × | × | × |
| 726–983a | Unknown | × | × | ||
| 833 | CH2 rock, α-phase90 | × | × | × | × |
The CI of PA6 can be calculated by the IR absorbance ratio of the C
O stretch, at 1637 cm−1, and a reference peak. Reference peaks are selected based on their independence of chemical changes, and for PA6, this is the peak associated with the Brill transition at 1124 cm−1.82 However, because of the overlapping spectral peaks arising from weathering that occur in this region, deconvolution of the peak at 1124 cm−1 was not possible.
Interestingly, similar to PS, PA6 weathered in artificial seawater and Puget Sound seawater did not produce as many new IR peaks. The salt in these two weathering conditions may hinder the degradation effects of PA6 in a similar manner to PS, where reactive chlorine radicals
quench perhydroxyl radicals
.45 In terms of PA6, the chlorine radicals may disrupt other reactive oxygen species, such as OH and
, that contribute to the degradation process.94 This is an interesting finding as aquaculture and fishing regularly utilize PA in their equipment, and our findings suggest there is more to understand about the photodegradation of lost fishing lines, also known as ghost fishing, in the marine environment. Previous work found that PA6 could not be degraded by microorganisms and will generally remain in the environment until they are photooxidized and mechanically crushed into microplastics.95
Comparing these findings reveals key polymer-specific behaviors. Unlike PE and PP, PS showed stability in its Raman spectra under all conditions, while its IR spectra were altered by oxidation, especially in DI water, where unique byproducts formed. PET primarily showed increased structural disorder (D-band) via Raman, particularly in water, and accumulated more oxidative byproducts (IR) when weathered in air. PA6, like PS, was relatively stable but also produced more unique IR peaks in DI water compared to seawater. The contrasting effect of seawater on PE and PP compared to more functional group containing polymers such as PS, PET, and PA6 highlights the complex interplay between polymer structure and environmental chemistry. These distinct pathways underscore the need for polymer-specific analyses and the use of complementary spectroscopic techniques (Table 6). While bulk factors such as Flory–Huggins or Hansen solubility parameters are often used to describe polymer–solvent interactions, they do not account for the non-linear trends observed here. For instance, PE and PP would be expected to degrade less in seawater due to their hydrophobicity and yet they show significant spectral change.
| IR | Raman | |
|---|---|---|
| PS | No major changes observed in air weathering; water conditions showed multiple weathering bands; water weathering effects can obscure identifying peaks | No change; all identifying peaks observable |
| PET | Observation of broad OH band formation; identifying peaks still observable | Formation of peak around 1352 cm−1 |
| PA6 | Observation of broad OH band and presence of some peak formations in the fingerprint region | Identifying peaks are observable, though peak intensity may differ |
It is important to note that complementary spectroscopic techniques, such as IR and Raman, have challenges and limitations when used in environmental microplastic analysis. These spectroscopic techniques support each other in confirming the identification of weathered microplastics and can provide microplastic researchers with information on some properties of the weathered materials found in the environment. While laboratory conditions can be easily controlled and manipulated, they do not truly reflect the degree of interaction that microplastics undergo in the environment. Therefore, it is important that laboratory experiments take into consideration multiple interacting factors that influence weathering. Additional techniques, such as DSC or XRD, should be integrated into future workflows to bridge the gap between surface-level spectral observations and bulk morphological transitions, to provide a more holistic understanding of the origin of these weathered structural changes.
Supplementary information (SI): representative IR and Raman spectra of PS, PET, and PA6, and carbonyl index analyses are included. See DOI: https://doi.org/10.1039/d5sm01102g.
Footnote |
| † Current address: pi-Conjugated Polymers Unit, Okinawa Institute of Science and Technology, Onna, Okinawa 904-0495, Japan. E-mail: christine.luscombe@oist.jp |