Sofía
Antic Gorrazzi
a,
Diego
Massazza
a,
Andrea
Pedetta
a,
Leonel
Silva
b,
Belén
Prados
c,
Gastón
Fouga
c and
Sebastián
Bonanni
*a
aDivisión Ingeniería de Interfases y Bioprocesos (IIBio), INTEMA. Av. Colon 10850, Mar del Plata (7600), Argentina. E-mail: sebastian.bonanni@fi.mdp.edu.ar
bDivisión Ciencia e Ingeniería de Polímeros, INTEMA. Av. Colon 10850, Mar del Plata (7600), Argentina
cInstituto de Energía y Desarrollo Sustentable, Centro Atómico Bariloche, CNEA, Av. E. Bustillo 9500, 8400 S. C. de Bariloche, Rio Negro, Argentina
First published on 24th May 2023
Biochar has emerged as an attractive electrode material due to its biocompatibility, low cost and reduced environmental impact. The temperature at which biochar is produced greatly affects its physicochemical properties and its environmental performance. Despite that, only biochar obtained at relatively high temperatures (800 to 1000 °C) has been applied in microbial electrochemical technologies (METs) so far. In this work, the physicochemical and electrical properties of biochar electrodes obtained at several temperatures (500 °C to 1000 °C) are explored and compared to those of graphite which is the most commonly used electrode material in METs. Besides, the associated carbon emissions and energy input of the production process at each temperature are estimated and compared to those of graphite. Results indicate that low-temperature (600 °C) biochar electrodes generate about half of the electric current obtained with high-temperature biochar or graphite electrodes. Furthermore, carbon emissions and energetic inputs for the production of low-temperature biochar are much lower than those of graphite production, with the 600 °C electrodes having a net positive carbon footprint and also a lower production cost. Nevertheless, further research is needed to optimize biochar conductivity and mechanical performance in order to allow its integration into large scale METs.
Sustainability spotlightAs stated in the UN's Sustainable Development Goals (SDG12 and SDG13) the application of sustainable patterns of production including the reduction of material footprint and greenhouse gas emissions is essential for mitigating climate change and lowering biodiversity loss and pollution. Electrochemical grade graphite production is based on the extraction of mineral ores and fossil fuels and is associated with high energy inputs and carbon emissions. In this work we study the use of biochar obtained from pruning residues as an alternative to graphite in bioelectrochemical systems showing that this material has an acceptable performance and, more importantly, requires low energy input for its production and can have a net positive carbon footprint. |
Electrode materials play a crucial role in MET performance and cost.2 The high cost of the electrodes represents a major drawback of microbial electrochemical technologies and the identification of cheap materials is essential for allowing the scale-up and commercialization of METs.3 Hence, the study and development of efficient and cost-effective electrodes is a very active research field.4
Graphite is the most widely used electrode material in METs due to its excellent electrochemical properties, biocompatibility, chemical stability and the variety of forms in which it is commercially available (rods, fibre brushes, granules, carbon-fibre cloths, paper sheets and felts, among others).5
Graphite is one of the crystalline forms of carbon and can be obtained either through mining of natural ores or through synthetic means.6 Its content in the ore from which this material is obtained in nature varies between 5 and 40% by weight. In order to achieve the purity needed for electrochemical application, mechanical separation of graphite from the ore and chemical and/or thermal post-treatments are required.6 On the other hand, synthetic graphite is obtained commonly from petroleum coke or coal pitch, through a high energy demand process that, among several steps (calcination, crushing, baking, impregnation), involves heating unstructured carbons to temperatures above 2500 °C in order to generate a crystalline structure.
The non-renewable nature of the raw materials of both natural and synthetic graphite, as well as the high energy demand and associated carbon emissions of its manufacturing processes, makes graphite a non-sustainable electrode material. Furthermore, due to the complexity of the required equipment, electrochemical grade graphite has a high cost that may rise in the near future due to the increasing demand for its application in Li-ion batteries for electric vehicles. Alternative materials for replacing graphite with lower manufacturing costs, higher availability and lower environmental impact must thus be investigated.
Biochar has emerged as an attractive electroconductive and biocompatible material due to its low cost and reduced environmental impact. It is conventionally obtained by subjecting biomass to reductive pyrolysis, which consists in heating in an anoxic atmosphere. Feedstocks used for biochar production are diverse and include lignocellulosic matter such as wood chips and pellets, husks, and forestry and crop residues, as well as alternative biomass sources such as sewage sludge, poultry litter, dairy manure and bones.7
Besides allowing waste valorisation, biochar has a high carbon content of up to 90% by weight.7 This carbon forms stable chemical structures that, according to recent estimations, may last between 90 and 1600 years in the material.8 In this way, CO2 emissions that would have been produced if biochar feedstocks were subjected to composting or incineration are avoided. Consequently, biochar production stands as an emerging carbon sequestration strategy.9
In addition, biochar is widely used as fuel for combustion,10 as a soil amendment to improve crop yield11,12 and as an adsorbent for the removal of contaminants from drinking water and wastewaters.13 Recently, it has been applied in biological wastewater treatment systems such as anaerobic digesters14,15 and treatment wetlands.16–18 In such systems, biochar improves several aspects: it boosts microbial activity by allowing electron exchange between microbial species, it increases the buffer capacity of the liquid media and it can be used as a substrate for biofilm growth.
Recently, biochar has been applied as an electrode material in microbial electrochemical technologies.5,19–21 As an electrode material, it has shown improved efficiency when compared with traditional graphite electrodes in terms of produced power,22–24 projected current density19,20,25 and volumetric current densities.25 Biochar was also used as a base material for improving oxygen reduction on cathodes.26
The electric conductivity and the porosity of biochar, properties of great importance for its application in electrochemical systems, are strongly dependent on the temperature of pyrolysis, which usually ranges between 350 and 1000 °C.7 Furthermore, the energy input, carbon emissions and production cost of the material as well as the complexity and cost of the equipment needed for its production are also highly dependent on the processing temperature. Despite this, only high temperatures ranging between 800 and 1000 °C have been used so far for obtaining biochar for MET electrodes.27,28
In this work, biochar electrodes of controlled area obtained at different temperatures with Cyperus papyrus as feedstock were used as electrode materials for the growth of electro-active bacteria. Compared to other macrophytes with similar characteristics, this species is commonly applied in treatment wetlands, requiring an annual pruning that generates large amounts of solid residues. The macrophytes' characteristic shape with elongated, cylindrical stems and a relatively uniform diameter along their length make them attractive for application as electrode materials allowing the revalorization of pruning residues.
The current produced by Geobacter sulfurreducens on biochar electrodes obtained at different temperatures was compared to that produced on graphite. It was found that more than half of the electric current obtained with graphite electrodes can be produced with low temperature biochar electrodes (600 °C). Furthermore, lowering the temperature of biochar production reduces both the associated energetic input and carbon emissions, with low temperature (600 °C) biochar having a net positive carbon footprint. Besides, cheaper equipment can be applied for obtaining biochar at low temperature, reducing the cost of the material.
Further research is needed to optimize biochar properties such as conductivity and mechanical performance to allow its integration into large scale METs. Nevertheless, due to the low cost and favourable environmental impact of low-temperature biochar this is an interesting challenge that may allow improvement in the applicability and sustainability of microbial electrochemical technologies.
From now on E500, E600, E800 and E1000 will be used to refer to electrodes obtained at 500, 600, 800 and 1000 °C, respectively.
The stable current density (j) of each working electrode was calculated from the individual current of each electrode divided by their arithmetic area. For the biochar electrodes, the area measurements were performed with ImageJ software.
The values of current density from each electrogenic culture assay included in a range of ±SD (N = 4 for E600 and graphite and N = 3 for the others) were statistically analyzed. Normality of the data set was analyzed using the Shapiro–Wilk test. After confirming normality, Fisher's F-test was performed to analyze the homoscedasticity of the samples and two-tailed Student's t-test. The significance level was 0.05 (p-value).
The integrity of the extracted DNA was checked by electrophoresis on a 1.2% agarose gel. DNA quantification (ng DNA per μl of sample) was analyzed with a NanoDrop spectrophotometer. Since low-temperature biochar can interfere with DNA quantification because of the presence of functional groups on its surface,36 DNA quantification of E500 and E600 electrodes was performed directly from the gel using ImageJ software. The ratio between the concentration obtained from the gel for the biochar and graphite electrodes was multiplied by the concentration measured for graphite electrodes with the Nanodrop spectrophotometer to calculate the DNA concentration in E500 and E600 samples. The number of bacteria (NB) was obtained from the DNA content of a single bacterium determined by quantification of total DNA from samples of known bacteria density (1 × 107 cells per μgDNA).
Several changes in biochar composition, structure and conductivity occur with increasing pyrolysis temperature.39 Consequently, variations in electric current production are expected among biochar electrodes obtained at different temperatures.
During pyrolysis, the feedstock is subjected to a complex set of chemical reactions that include the condensation of aliphatic and aromatic compounds in conjugated structures and the release of volatile molecules (alcohols, oils, tar), methane, carbon monoxide and hydrogen.40 The extent to which these reactions proceed is largely determined by the temperature of the heat treatment process.41 At relatively low temperatures (between 300 and 600 °C) liquid and tar forming reactions prevail. At temperatures above 600 °C the removal of oxygen, nitrogen and sulfur as well as condensation reactions becomes increasingly important. Consequently, the oxygen content of biochar samples decreased with pyrolysis temperature (see ESI†).
Among the oxygenated chemical compounds of biochar, quinone-like compounds are one of the most prevalent.42 These components have CO bonds that, being formed by atoms of different electronegativity, generate regions of differential charge density on its structure. In accordance with the decay in oxygen content, FTIR assays showed a decrease in the concentration of quinone-like components with increasing pyrolysis temperature (see ESI†).
In contrast to oxygen, the carbon content of biochar increased with pyrolysis temperature. This occurs because during condensation reactions (that become increasingly important at higher temperatures) carbon becomes part of the stable and highly conjugated aromatic compounds. In these compounds, the carbon atoms form a local crystalline structure resembling that of graphite, with stacked flat aromatic sheets that are randomly cross-linked.43
Biochar also has inorganic moieties. The inorganic fraction of biochar electrodes was mainly formed by sodium, potassium, calcium and magnesium salts that, according to elemental analysis, showed increasing content with pyrolysis temperature (see ESI†), as previously reported.12 The ash content of E1000 biochar was 12.4 ± 0.7%, whereas the ash content of the feedstock was 6.0 ± 0.5%. No ash was obtained on graphite samples. The results of TGA in an oxygen atmosphere for graphite and E1000 are shown in the ESI.† Salts were detected only in raw biochar samples and not in samples used as electrodes in electrochemical cells, most likely due to their solubilization in the liquid media.
Despite the observed changes in biochar composition, the zeta potential which is used as an indirect measure of the surface charge of particles44 was similar for all samples (see ESI†), suggesting the existence of similar charge densities on the surface of the electrodes.
The increased molecular order of the pyrolyzed biomass gives it a higher mechanical strength than the feedstock from which it was derived.43 Despite this, the biochar produced in this work had similar mechanical strength at all temperatures. Mean resistance to compression was 0.63 ± 0.08 MPa, which is much lower than that of graphite (4.70 ± 0.71 MPa). Strategies such as densification of the obtained biochar with pyrolysis oil or other binders,45 or the selection of harder feedstocks such as those with high lignin content, may be plausible alternatives to increase biochar's mechanical strength and to improve its applicability of biochar electrodes on large scale systems.
Chemical compounds in low-temperature biochar (e.g. quinones) may serve as electron acceptors for electro-active bacteria (see ESI†).46 Nevertheless, the electric current obtained with E500 electrodes was very similar to the current prior to inoculation (blank), indicating that little or no bacterial growth was caused by these electrodes.
The E800 and E1000 current density values were similar to those of graphite electrodes, whereas intermediate current densities were obtained with E600 electrodes (Fig. 1A).
Fig. 1 (A) Electric current density (j) produced on E500 (yellow), E600 (orange), E800 (red), E1000 (dark red) and graphite (black) electrodes by G. sulfurreducens cells. Base currents were subtracted. Letters on the bars indicate statistically significant differences between electrodes (p < 0.05). N = 4 for graphite and N = 3 for the other electrodes. (B) Electric current density (j) as a function of relative graphitization (calculated as the ratio between G and G + D peak areas of the Raman spectra, see ESI† for details) for biochar electrodes and graphite. The dotted line represents the fitting with an asymptotic function. (C) Electroconductivity (S cm−1) of different biochar and graphite electrodes (N = 2). |
The differences in obtained current densities are explained by structural changes promoted by high pyrolysis temperatures. Graphitization was analysed by Raman micro-spectroscopy (see ESI†). Raman spectra suggest that E500 was formed mainly by amorphous (disordered) carbon, whereas higher temperature biochar showed a progressive decrease in the disorder and an increase in the degree of graphitization, as previously reported for other feedstocks.47–49
The current density produced by the bacteria highly depended on the degree of graphitization of the electrodes (estimated here from the fraction of total peak area represented by graphitic peak G, see ESI†). These two variables showed an asymptotic relation (Fig. 1B). In this context, the graphitization degree may be a useful parameter to preliminarily determine whether the biochar obtained from different feedstocks and under different pyrolysis conditions could be used as an electrode material for electro-active bacteria growth.
Graphite crystallites are formed by organized clusters of sp2 hybridized atoms. As the π electrons of sp2 carbons are responsible for the electrical conductivity of biochar, the graphitization degree highly influences the conductivity of the material.49 As a result of the higher degrees of graphitization shown above, higher conductivities were obtained with increasing pyrolysis temperatures (Fig. 1C). The conductivity of the material exhibited a significant increase when the pyrolysis temperature was raised from 500 to 600 °C. At higher temperatures, a progressive enhancement in conductivity was observed, with the materials pyrolyzed at 1000 °C having conductivities within the same order of magnitude as that of graphite.
Electrode conductivity is of great importance for MET efficiency as it determines the potential sensed by the bacteria at the electrode/solution interface. When growing bacteria on three-electrode cells as those used in this work, a potential is applied at one end of the working electrode with a potentiostat, but the actual potential at the face of the electrode submerged on the liquid media may differ from the applied value, since the electron flow through the electrode generates a potential drop. Consequently, if the electrode is not sufficiently conductive, the real potential may not be favourable for bacterial respiration, interfering with the generation of electric current.
Taking the mean produced current densities at each electrode and the respective electric conductivities, potential drops across the biochar material of 350 mV, 40 mV and 0.4 mV were estimated for E600, E800 and E1000 respectively. As the applied potential to the working electrode was 0.2 V vs. Ag/AgCl, it can be estimated that the actual potential at the electrode/biofilm interface was −150 mV, 260 mV and 199 mV vs. Ag/AgCl for each of these electrodes. Considering that the lowest potential value at which G. sulfurreducens can use an anode as electron acceptor is around −0.45 V vs. Ag/AgCl, these values indicate that the actual potential applied to the electrodes was favourable for bacterial respiration in all cases.
On the other hand, a much higher potential drop was estimated for the E500 electrodes (close to 1.2 V). This indicates that the real potential on the submerged face of the E500 electrodes was unfavourable for bacterial respiration, and that the low amount of current obtained on these electrodes was not related to bacterial respiration.
To gain further insight into the relationship between current and applied potential, cyclic voltammetry was performed (Fig. 2). In accordance with the higher conductivity of the electrodes, the CV signals of the E800 and E1000 electrodes were similar to that obtained with graphite.
In these cases, electric current production started at potentials of around −0.45 V vs. Ag/AgCl and showed a sustained increase with the applied potential. This current increase is produced by an acceleration of bacterial metabolism due to the increasing oxidation of redox intermediates acting between the bacteria and the electrode.50 Once a potential of around −0.2 to −0.1 V vs. Ag/AgCl was applied, cells were working at the maximum rate and electric current reached a stable value.
Signals of E600 showed a different behaviour, not reaching a stable current value even at the highest applied potential. As shown above, E600 electrodes had a lower (and possibly heterogeneous) conductivity than E800 and E1000 and, consequently, there may have existed areas where the actual electrode potential was below the values needed for optimal bacterial activity. In this context, despite allowing the production of a relatively high current density on the three-electrode cell configuration used in this work where the electrode length was small (∼1 cm), the relatively low conductivity of the E600 electrode may preclude its application in systems where electrons have to be transported across longer distances, such as large-scale microbial fuel cells and microbial electrolysis cells. In fact, for these systems it has been stated that even graphite electrodes lack the appropriate conductivity for avoiding considerable ohmic drops. The application of current collectors was identified as a crucial design aspect for reducing ohmic drops and allowing an efficient scale up.51 They would necessarily have to be applied when using biochar electrodes.
SEM images show that bacteria did not colonize the internal pores of the material (see ESI†) and were only found on the surface of the electrode, where they formed thick biofilms that covered even the larger pores of the material (Fig. 3). Nevertheless, the coverage of the 600 °C electrodes was not as homogeneous as that of the graphite electrodes. On those electrodes, biofilms had heterogeneous thickness, with some regions being covered by less than a monolayer (Fig. 3(D1)). This suggests that some parts were not favorable for electrode respiration by the bacteria, possibly due to particularly unfavorable potentials produced by heterogeneities in the conductivity of the electrode and/or the composition of the biochar. These heterogeneities may have reduced the current generated by the bacteria on certain portions of the electrode, explaining the lower respiration rate estimated above for these electrodes.
Natural graphite is mined in open and underground pits and ore has low graphitic carbon content (2 to 30% by weight). In order to achieve the high purity (>99%) needed for its application in electrochemical devices, several beneficiation steps are required, including milling, flotation, leaching, roasting and thermal processing. Most of the energy demand of these processes is delivered from the combustion of fossil fuels, with the remaining 20 to 25% coming from electricity.52
Graphite can also be synthetically produced through what is known as the Acheson process. The most common feedstock for this process is coke, a solid material with high carbon content that derives from oil refining and cracking of heavy oils. To obtain graphite, coke must be calcined to remove volatile compounds and then subjected to a graphitization step that involves heating to temperatures above 2500 °C for about 3 to 5 days, commonly in electrically heated furnaces.
Further processing steps may involve grinding, impregnation with a binder and baking at temperatures between 800 and 1500 °C.
Consequently, the production of electrodes from both synthetic and natural graphite is energy intensive.52 The estimated energetic input for natural graphite production ranges between 43.8 MJ kg−1 (ref. 53) to 112.48 MJ kg−1 (ref. 54) whereas the synthetic graphitization process has an estimated input of 45.9 MJ kg−1 (ref. 52).
Much lower energy is required to produce biochar through pyrolysis. Traditionally, biochar is applied as a soil amendment or for bioenergy production through combustion. For these applications, biochar is commonly obtained at temperatures ranging between 350 and 500 °C. As pyrolysis is an exothermic process and releases gases that can be combusted, a small amount of energy which is estimated to be 0.058 MJ kg−1 is only needed during initial start-up of the pyrolysis kiln.55
The production of biochar for its application as an electrode material is different from the traditional approach, as higher temperatures are required. Anyway, as will be shown, the energy requirement of the process is still much lower than that of graphite production. An estimation of the energy requirement of the pyrolysis will be performed by considering the production of biochar in an electric industrial oven. A heating ramp of 10 °C min−1 (like that applied in this work), an initial temperature of 20 °C and a pyrolysis time (at final temperature) of 60 min are considered. Also, the energy demand of a static chamber furnace that can handle 1.5 m3 (750 kg of bulk material) per batch is considered (96 kW for Carbolite SBCF-3/11/1700). Considering these values and taking a mass yield of 30% like that obtained in this work (see ESI†), an energy demand of 3.0, 3.53 and 4.05 MJ kg−1 can be estimated for pyrolysis temperatures of 600, 800 and 1000 °C respectively.
Other steps in biochar manufacturing rather than pyrolysis also consume energy, with drying being the most important when using vegetables residues as feedstock. Depending on the feedstock and its initial water content, these steps can consume from 0.35 to 2.45 MJ kg−1.56 Taking the mean between these values together with the estimations for the pyrolysis process, the total energetic input for obtaining electrodes at 600, 800 and 1000 °C from vegetable residues can be estimated to be 4.40, 4.93 and 5.45 MJ kg−1 which are an order of magnitude lower than the estimations for graphite production. It has to be taken into account that if plants cultivated with the sole purpose of being used for biochar production are used as feedstock instead of vegetable residues, other energy demanding concepts should be considered in the process, such as the production of agrochemicals needed for plant growth and harvesting operations, which may account for up to 1.1 MJ kg−1 additionally.56
A low energetic demand is related to lower CO2 emissions into the atmosphere, especially if the required energy is generated through fuel combustion. Taking as a reference the mean emissions of USA's electric energy grid, 0.57 kg CO2 per kW h,57 it can be estimated that emissions of the pyrolysis process are about 0.48, 0.56 and 0.64 kg CO2 per kg for E600, E800 and E1000. Other sources of CO2 emissions on the biochar production process are the production of agrochemicals, field operations and changes in land use related to feedstock cultivation, which together can be between 0.08 and 1.03 kg CO2 per kg.56 As previously mentioned, these latter emissions can be neglected if vegetable residues are used as feedstock.
Furthermore, it has to be considered that most carbon in biochar is in a highly stable state and, as a consequence, biochar can be used for carbon sequestration. As the carbon content of biochar obtained from plants and wood is about 70% by weight7 and 80% of carbon in biochar is in stable form,56 it can be estimated that biochar's carbon sequestering capacity is about 0.56 kg CO2 per kg.
Notably, this estimation and the emissions estimated above suggest that E600 electrodes may have a positive carbon footprint of about 0.08 kg CO2 per kg. This represents a great advantage of E600 electrodes in comparison with those obtained at higher temperatures and specially with graphite, a material whose production is related to high carbon emissions into the atmosphere ranging between 2.15 (ref. 53) and 5.3 kg CO2 (ref. 54) per kg of graphite for the production of electrodes from natural graphite and reaching 13.8 kg CO2 per kg of graphite (ref. 13 and 52) for its synthetic production.
Besides affecting the energy input and net carbon emissions, pyrolysis temperature also affects the cost of the equipment needed for the thermal treatment. Special nickel based alloys are needed for processes at high temperatures, whereas iron based materials and aluminium alloys can be used for lower temperatures up to 600 °C. Nickel based alloys are much more expensive than iron and aluminium and, as a consequence, high temperature ovens are much more expensive than low temperature ones that can be constructed with iron based materials such as stainless steel.58 Estimations show that the equipment for achieving temperatures close to 1000 °C is almost 6 times more expensive than that for achieving temperatures lower than 650 °C.59 Considering the cost of the energy and the depreciation of the equipment needed for biochar production, it was estimated that the cost for obtaining biochar at 600 °C is three times lower than for the production at 1000 °C.60
Biochar electrodes still have some limitations that have to be overcome to allow their effective application. The low conductivity is a major drawback of biochar electrodes as the material, even when obtained at high temperatures, still lacks the needed electrical conductivity to allow electron transfer over long distances. Consequently, as noted previously for graphite electrodes, biochar electrode designs may have to incorporate metals as current collectors to allow their application in large scale systems. Obtaining higher conductivity electrodes at low pyrolysis temperature is a major challenge that may be addressed through the study of different feedstocks and the analysis of different pre-treatments.
Also, the mechanical strength of biochar must be improved for enhancing the applicability of biochar electrodes. Strategies such as densification with pyrolysis oil or other binders and the use of alternative feedstock with improved mechanical properties may be plausible strategies to achieve such improvement.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3su00041a |
This journal is © The Royal Society of Chemistry 2023 |