Cornelius A.
Obasanjo
a,
Ali Shayesteh
Zeraati
b,
Hadi Shaker
Shiran
b,
Tu N.
Nguyen
ac,
Sharif Md.
Sadaf
d,
Md Golam
Kibria
*b and
Cao-Thang
Dinh
*a
aDepartment of Chemical Engineering, Queen's University, Kingston, ON K7L 3N6, Canada. E-mail: caothang.dinh@queensu.ca
bDepartment of Chemical and Petroleum Engineering, University of Calgary, 2500 University Drive, NW Calgary, Alberta T2N 1N4, Canada. E-mail: md.kibria@ucalgary.ca
cHelen Scientific Research and Technological Development Co., Ltd, Ho Chi Minh City 700000, Vietnam
dCentre Energie, Matériaux et Télécommunications, Institut National de la Recherche Scientifique (INRS)-Université du Québec, 1650 Boulevard Lionel-Boulet, Varennes, Quebec J3X 1S2, Canada
First published on 19th July 2022
The valorization of carbon dioxide (CO2) via electrochemical CO2 reduction (ECR) has attracted great interest as a pragmatic approach to tackle greenhouse gas emissions. Multiple carbon (C2+) products, such as ethylene (C2H4), ethanol (C2H5OH), and propanol (C3H7OH), are highly valuable chemicals and of great demand. Copper (Cu)-based catalysts are so far the only electrocatalytic materials that allow CO2 reduction to C2+ products at industrially relevant current densities (≥100 mA cm−2). However, most Cu-based catalysts are unstable in long-term reactions (>100 hours), with the main reasons being the potential-induced surface reconstruction, deposition of impurities, and catalyst aggregation and leaching, among others. Herein, we report an in situ catalyst regeneration strategy that can extend the operation time of Cu-based catalysts. By periodically adding segments of anodic currents to electrolysis, a Cu catalyst is partially oxidized to CuOx in each cycle, as confirmed by in situ Raman studies, leading to the restoration of the catalytically active sites for C2+ products. We found that the oxidation current density and time significantly affect the selectivity and stability of Cu catalysts. Applying this strategy to a Cu catalyst – which is stable for ∼5 h towards C2+ products during a continuous electroreduction under neutral-pH conditions, we were able to extend the operating time to ∼120 h in a flow cell system. The catalyst maintained a high faradaic efficiency (FE) for C2H4 of ≥50% at a fixed cathodic current density of 150 mA cm−2 for over 60 h and continued to operate with a C2H4 FE ≥ 40% for the entire length of the reaction time. This work opens up an avenue to enhance the stability of Cu electrocatalysts, via controlling the operating procedure during electrolysis.
A wide range of electrocatalytic materials for ECR have been investigated and reported in the literature. Electrocatalysts with high selectivity (FE > 80%) and long-term stability (>100 h) when performing at industrially relevant current densities (>100 mA cm−2) have been reported for single carbon (C1) products such as carbon monoxide4–7 and formic acid/formate.8–10 Cu and Cu-based catalysts have drawn great interest for ECR studies, not only because of their natural abundance and low cost, but also due to their unique feature as the only catalysts capable of converting CO2 into valuable C2+ products at high current density.11–17 Recent improvements in Cu-based catalysts and cell design have promoted ECR at elevated current densities even beyond 1 A cm−2.14 In some cases, high selectivity under alkaline and neutral-pH conditions was achieved, with FE values in the range of 40–72% and 41–52% for C2H413,14 and C2H5OH,12,15 respectively. Interestingly some high-performing ECR Cu-based electrocatalysts with C2H4 ≥ 75%18,19 have also been demonstrated with stability ≤ 100 h and current density < 100 mA cm−2. Nevertheless, the reported stability of ECR has been limited to a few operating hours13,20,21 for these C2+ products. In most cases, the Cu-based catalysts are rapidly deactivated, particularly when ECR reactions are conducted in neutral-pH or acidic media, as the competing hydrogen evolution reaction (HER) prevails after a short period.22 Notably, performing ECR under alkaline conditions has previously been shown to extend the catalyst operating time while displaying good selectivity for C2+ products. However, under these conditions, CO2 directly reacts with KOH and forms bi/carbonate salts, necessitating additional energy expenses for electrolyte and CO2 regeneration.13 Thus, there is a need to design suitable electrocatalysts and/or devise electrolysis procedures that can stably produce C2+ products in neutral or acidic environments to make the ECR technology more economically competitive.
Improving the stability of Cu electrocatalysts in low pH media still remains a great challenge.20,23–26 A wide array of reasons for Cu catalyst electrode failure have been reported, including poisoning by reaction products,27 deposition of metal impurities from the electrolyte,28 potential-induced surface reconstruction exposing inactive facets,29–37 and dissolution and redistribution of the catalyst outer surface.38,39 For gas diffusion electrodes (GDEs), which allow ECR to operate at industrially relevant current densities, catalyst deactivation is also due to the flooding of the porous gas diffusion layer and the precipitation of bi/carbonate salts that block the transport of CO2 gas to catalytic sites. To address the instability of Cu-based catalysts, strategies such as pulse electrolysis25,26,40–42 or employing electrolytically-cleaned electrolytes have been reported.43 It is also worth knowing that pulsed ECR has also been extensively studied towards enhancing C2+ product selectivity.44–47 Pulsed potential electrolysis has been exploited towards enhancing the stability of Cu-based electrocatalysts. Jännsch Y. et al.26 used 25 s at −1.38 V and 5 s at −1.0 V (vs. Ag/AgCl) to increase the stability of C2H4 production from less than 8 h to at least 16 h. Engelbrecht A. et al.25 extended a 16 h potentiostatic electrolysis to about 85 h and 95 h via variation of cathodic pulse potential (tc = 25 s, ta = 5 s, Uc = −1.6 V, Ua = −0.18 V, vs. Ag/AgCl) in combination with two different modes of electrolyte management, respectively. They both achieved C2H4 FEs below 40% which were demonstrated at current densities below 100 mA cm−2. However, to the best of our knowledge, none of these approaches have been able to demonstrate long-term stability towards C2+ products with high FE and at a high reaction rate in a flow cell configuration.
Herein, we report an in situ surface regeneration strategy to extend the operating time of a Cu electrocatalyst in neutral-pH media. The strategy is based on previous observation that oxide-derived Cu (OD-Cu) catalysts are effective for selective CO2 reduction to C2+ products.48,49 We exploited the copper oxide formed during the regeneration step of a thoroughly optimized oxidation and reduction cycle to target an extended ECR to C2+ products. With this in situ regeneration strategy, we achieved an order of magnitude improvement in operating time, with the Cu electrode operating at a cathodic current density of 150 mA cm−2 for ∼120 h. It maintained FE values for C2H4 ≥ 50% for over 60 h and remained operating with C2H4 FE ≥ 40% for the entire reaction time.
Fig. 1 Characterization and ECR selectivity of Cu/PTFE. Scanning electron microscopy (SEM) images of Cu/PTFE with nominal Cu thicknesses of 200 nm (a), 700 nm (b) and 1000 nm (c). CO2 reduction product distribution at different cathodic current densities in 1 M KHCO3 electrolyte using Cu/PTFE with nominal thicknesses of 200 nm (d), 700 nm (e) and 1000 nm (f). The FE error bar was calculated based on data collected from different experimental trials (n = 3). Potential data for the determination of ECR selectivity of Cu/PTFE for all samples are provided in the ESI (Fig. S3).† |
ECR performance of Cu/PTFE GDEs was evaluated with a flow-cell reactor using 1 M KHCO3 catholyte. A bipolar membrane was used to separate the anode and cathode compartments. Nickel (Ni) foam and 1 M KOH solution were used as the anode and anolyte, respectively. The ECR of Cu/PTFE catalysts was studied in the cathodic current density range of 100–250 mA cm−2 using chronopotentiometry. Gaseous products were analyzed with in-line gas chromatography while liquid products were collected and analyzed using nuclear magnetic resonance (NMR) (Fig. S2†). All Cu/PTFE samples showed FE values for C2H4 between 38 and 55% in the studied current range, with a total C2+ (C2H4, C2H5OH, C3H7OH, and C2H3O2−) FE of >70% achieved at current densities of 150–250 mA cm−2 (Fig. 1d–f). This performance is consistent with previous reports on Cu/PTFE catalysts using similar testing conditions.21,50 We observed that Cu thickness showed little impact on the overall product selectivity within the explored current density range. While the total C2+ was lower at 100 mA cm−2 for all Cu/PTFE samples, the value increased about 15–20% at current densities between 150 and 250 mA cm−2. At these higher current densities, the Cu/PTFE GDEs maintained a good C2+ FE of >70%. However, at current densities beyond 300 mA cm−2 we observed a decrease in the total C2+ FE with a corresponding increase in H2 and CH4. The FE value of CH4 was found to be the highest on the 200 nm Cu/PTFE sample and was approximately 10 times higher at all current densities explored. These results suggest that the thickness of Cu/PTFE can be optimized to either achieve a high FE for C2+ products (thick Cu/PTFE) or a high FE for CH4 (thin Cu/PTFE).
To study the stability of the GDEs, we performed the ECR reaction at a fixed current density of 150 mA cm−2 and analyzed the gaseous products over time. The thickness of the Cu layer had a significant effect on the stability of Cu/PTFE. For the 200 nm Cu/PTFE, the C2H4 FE was stable at around 50% for about 1 h before it started decreasing rapidly, reaching 15% after 1.5 h of continuous reaction (Fig. 2a). After 1 h of reaction, the FE values of both CH4 and H2 started increasing, with H2 being the dominant product after 1.5 h (Fig. 2a–c). The stability of Cu/PTFE catalysts was significantly improved with an increase in Cu nominal thickness. The 1000 nm Cu/PTFE maintained a C2H4 FE of 50% for 5 hours (Fig. 2a). For all Cu/PTFE samples, CH4 and H2 were the two main products when the C2H4 FE started decreasing (Fig. 2b and c), while CO selectivity slowly decreased over time (Fig. S4†).
Fig. 2 Stability of Cu/PTFE in ECR. Variation of gas products over reaction time at a constant current density of 150 mA cm−2 in 1 M KHCO3 electrolyte: (a) C2H4, (b) CH4 and (c) H2. SEM images of Cu/PTFE catalysts with a nominal thickness of 1000 nm before (d) and after continuous electrolysis for 7 hours (e). High resolution Cu 2p XPS spectrum of Cu/PTFE catalysts after continuous ECR tests showing the presence of metallic Cu, copper oxide and copper hydroxide (f). Chronopotentiometric plots for the three samples are provided in the ESI (Fig. S5–S7).† |
Previous studies on the stability of Cu catalysts for ECR in aqueous electrolytes have identified three main deactivation mechanisms among others. First, the Cu surface undergoes a reconstruction process, exposing the Cu sites (e.g. (111) facet) that are more selective towards CH4 formation and H2 production.51 This surface reconstruction usually occurs on the sub-10 nm scale. Second, metal impurities such as Fe and/or Ni present in the electrolyte, which can be deposited on the surface of Cu catalysts during electrolysis, form highly active sites for H2 production.52 The last mechanism involves the reduction of oxidized Cu species (Cu+, Cu2+) in Cu-based catalysts during the ECR process. Because oxidized Cu species and/or sub-surface oxygen are critical for CO2 reduction to C2+ products, the disappearance of these species makes the catalyst less selective toward C2+ products over time.53–55 Furthermore, for gas-phase ECR in flow systems using gas diffusion electrodes, the flooding of the gas diffusion layer and the precipitation of bi/carbonate salts can block the diffusion of the CO2 reactant, leading to the suppression of CO2 reduction.3
To identify the deactivation mechanism in our system, we first checked if flooding and salt precipitation were the main reasons. ECR at 150 mA cm−2 was performed continuously until the C2H4 FE decreased to around 25%. The current density was then reduced to 125, 100, 75 and 50 mA cm−2 and the gaseous products were analyzed accordingly. The FEs for H2 and CH4 remained high with lowering the current density, implying that CO2 diffusion limitation was not the reason for the drop in C2H4 FE (Fig. S8†). To further confirm that flooding was not the major mechanism for the deactivation of our Cu/PTFE sample, we investigated electrode flooding in our flow cell system using a capacitance change measurement.56 We quantified the electrochemical double-layer capacitance in an attempt to track the ingress of the electrolyte into the GDE during electrolysis. This capacitance measurement obtained through the cyclic voltammetry technique, in the non-faradaic region with variable scan rates, can offer insights into the changes that occurred at the electrode–electrolyte interface. The cyclic voltammetry was carried out between −0.05 V and −0.20 V vs. Ag/AgCl with scan rates of 10, 50, 100, 150 and 200 mV s−1. We observed no significant change in the electrochemical double-layer capacitance (Fig. S9–S11†). The capacitance was found to be around 0.5756 mF cm−2 at the open circuit potential before the start of continuous electrolysis, 0.5309 mF cm−2 after 3 h of electrolysis and 0.5143 mF cm−2 after approximately 6–7 h of continuous operation (Fig. S11†). The FE of C2H4 was about 56% after 3 h and decreased to about 42% at the end of the continuous operation.
To check for a change in the catalyst surface morphology, we compared the SEM images of the Cu/PTFE sample before and after continuous ECR tests (Fig. 2d and e). The surface texture of Cu/PTFE appeared to change after the reaction as the particle size became smaller. While this could be due to the surface construction, it may also have originated from the oxidation of the Cu surface when the sample was exposed to air after the reaction. High resolution Cu 2p X-ray photoelectron spectroscopy (XPS) of the sample (1000 nm) shows the presence of CuO and Cu(OH)2 after the reaction (Fig. 2f). The survey XPS spectra show no peaks for Fe and Ni in all samples while small peaks of C, F and Cl were detected (Fig. S12†). These data suggest that impurity could not be the main cause of lower C2H4 selectivity. We therefore reason that surface reconstruction and changing of the Cu oxidation state and sub-surface oxygen could be the main contributors to the deactivation of Cu/PTFE catalysts.
To investigate the recovery of Cu catalyst selectivity toward C2H4via in situ electrochemical oxidation, we first performed continuous ECR tests at a current density of 150 mA cm−2 until the C2H4 FE decreased to around 10–15% (Fig. 3a). Next, we performed repeated oxidation–reduction cycles until a stable C2H4 FE was achieved (Fig. 3a). The oxidation current density was varied between 0.4 and 1 mA cm−2 while the reduction current density and time were fixed at 150 mA cm−2 and 5 min, respectively. The FE of C2H4 was analyzed at the end of each reduction cycle. The oxidation time was studied to maximize C2H4 FE. In all cases, the oxidation charges (Q = I × t) explored were either 36, 24, or 12 mC. As shown in Fig. 3b–e, the C2H4 FE increases after each oxidation–reduction cycle while the FEs for H2 and CH4 slowly decrease (Fig. S13–S16†). The FE for CO remains relatively constant with the oxidation–reduction cycle (Fig. S13–S16†). C2H4 FE values >50% were achieved at all oxidation current densities, with higher applied charges allowing the catalysts to operate with higher C2H4 FE for each oxidation current density. This suggests that a higher oxidation current density only needs a shorter time to recover the high FE for C2H4.
Fig. 3 Regeneration of Cu catalysts by in situ oxidation. (a) Oxidation–reduction program for the recovery of C2H4 FE. All samples were operated continuously at a fixed reduction current density of 150 mA cm−2 until the C2H4 FE decreased to around 10–15%. The catalysts were then subjected to 20 repeated oxidation–reduction cycles. Each oxidation–reduction cycle involves an oxidation step at a designated current and time, followed by ECR at 150 mA cm−2 for 5 minutes. The gas products were analyzed at the end of each reduction cycle. The recovery of FE for C2H4 is shown with oxidation current densities of 0.4 mA cm−2 (b), 0.6 mA cm−2 (c), 0.8 mA cm−2 (d) and 1 mA cm−2 (e) at different oxidation periods. The dependence of maximum C2H4 FE on oxidation charge (f). The deviation was calculated based on data at different oxidation current densities but with similar oxidation charges (n = 4). The FE values for CO, H2 and CH4 during the oxidation–reduction cycle are provided in the ESI (Fig. S13–S16†). The morphology of Cu/PTFE after in situ electrochemical oxidation is presented in the ESI (Fig. S17†). |
The maximal FE for C2H4 was found to be a function of the oxidation charge regardless of the oxidation current density applied in our studied range (Fig. 3f) with a FE of 53–56% being recovered when the oxidation charge was ≥24 mC. In addition, at each given oxidation current density and time condition, we found that the C2H4 FE quickly recovered in the first 10 cycles before reaching a plateau. The presence of such a plateau suggests that (i) the 5 min ECR reaction after each oxidation step is not long enough to cause catalyst deactivation and (ii) the ratio between the catalytic sites for C2H4 and other products is dependent on the applied charge of the oxidation current density, which governs the final C2H4 FE.
Given the observed removal of adsorbed CO species and a significant drop in C2H4 formation, we performed in situ Raman studies using the oxidation–reduction strategy as a remedy against this deactivation. As the oxidation current density was applied, the Cu–CO and Cu–OH species disappeared, and the CuOx bands emerged in the range of 450–700 cm−1. These oxide species were visible after 20 s of oxidation current (Fig. 4b). The CuOx bands disappeared entirely while the Cu–CO and Cu–OH species reappeared after the reduction cycle. It has been shown that these CuOx crystals reduced into small Cu grains developing OD catalysts which facilitated the C–C coupling and accounted for enhanced C2H4 selectivity.63–65 Interestingly, by applying cathodic current the restricted rotation of adsorbed CO and Cu–CO stretching is recovered, confirming the re-coverage of CO. By repeating the oxidation–reduction cycles, more intense Cu–CO bonds were formed, which indicates enhanced CO coverage. Roldán Cuenya et al.63 showed that the intensity of ratio of the Cu–CO stretching band to the CO rotation band can be correlated to the CO coverage and a higher ratio leads to more C–C coupling and C2+ formation. Our SERS analysis illustrates an increasing trend of this ratio with increasing the number of oxidation–reduction cycles. This confirms a better CO coverage on the surface of the catalyst leading to the sustained C2H4 FE (Fig. S19†).
Fig. 5 Stability of the Cu/PTFE catalysts with the alternating current strategy. (a) Schematic illustration of the alternating current strategy. (b) Oxidation charge optimization at a fixed reduction current density of 150 mA cm−2 for 5 min reduction time. The cathodic potential versus time plot is provided in Fig. S21.† (c) Oxidation time optimization at a fixed current density of 150 mA cm−2 for 5 min reduction time and an oxidation current density of 1 mA cm−2 (the oxidation time was varied between 6 s and 36 s). The cathodic potential versus time plot is provided in Fig. S23.† |
To further explore the effect of the oxidation charge, we then fixed the oxidation current density at 1 mA cm−2 and varied the oxidation time from 6 to 36 s. The reduction current density and time are 150 mA cm−2 and 5 min, respectively. While larger oxidation charge leads to higher C2H4 FE, the catalyst becomes less stable when the oxidation time (oxidation charge) is increased (Fig. 5c). With a 36 s oxidation time, the catalyst showed the highest C2H4 FE of 54% but was stable at above 50% for 14–16 h before dropping quickly to about 30% in 20 h of operation. In contrast, when the oxidation time was reduced to 6 s, the catalyst operated stably for up to 75 h, although with a lower C2H4 FE of 40% and above (Fig. 5c). Under all operating conditions, the FE of CO slowly decreased while those of H2 and CH4 increased steadily with the reaction time (Fig. S22†). These results suggest that the oxidation time could not be tuned to achieve both high C2H4 FE and long stability simultaneously. While the catalyst can operate with an initial C2H4 FE of about 50% at all oxidation times, each operating condition tends to temporarily arrive at a constant FE as mentioned earlier, beyond which the cumulative effect of the total oxidation time over the catalyst operating lifetime begins to significantly impact the catalyst performance. Therefore, it can be hypothesized that the total amount of charge (the product of a given oxidation charge and the number of times it was cycled) throughout the lifetime of the operating catalyst determines the overall stability of the Cu/PTFE catalyst electrode.
To extend the lifetime of the catalyst, we turned our attention to the reduction time. We reason that if the stability of the catalyst depends only on the oxidation charge, the overall operating time can be extended by increasing the reduction time. We fixed the reduction current density (150 mA cm−2), oxidation current density (1 mA cm−2) and time (24 s) and varied the reduction time. As shown in Fig. 6a, increasing the reduction time extended the overall catalyst lifetime (time to maintain a C2H4 FE ≥ 40%). Based upon our optimized operating conditions, the longest catalyst lifetime of ∼120 h was achieved at a reduction time of 45 min. At this condition, the C2H4 FE was maintained at over 50% for more than 60 h, which is around ten times longer than the continuous operation (5 h). The CO FE decreased rapidly in the first 20 h and is then relatively stable (Fig. S24†). The CH4 FE slowly increased over time while the H2 FE varied in the range of 10–15% (Fig. S25 and S26†). Furthermore, under these operating conditions, we found that a further increase of the reduction time and/or oxidation charge does not improve the catalyst lifetime, at least for when we aim to maintain a C2H4 FE ≥ 40%. An operation of the catalyst under the same conditions, but with a higher oxidation charge (60 mC), was carried out for ∼58 h (Fig. S28†).
Fig. 6 Stability of the Cu/PTFE catalysts with the optimized alternating current strategy in 1 M KHCO3. (a) Reduction time optimization (varying from 5 to 45 min) at 150 mA cm−2 and a fixed oxidation current density and time of 1 mA cm−2 and 24 s, respectively. (b) SEM of Cu/PTFE after the oxidation–reduction strategy using 45 min reduction at a current density of 150 mA cm−2 and a fixed oxidation current density and time of 1 mA cm−2 and 24 s, respectively. The cathodic potential versus time plot is provided in Fig. S27.† |
A limited Cu catalyst lifetime with the optimized oxidation and reduction conditions implies a major deactivation mechanism different from the potential induced surface reconstruction and surface impurities discussed above. To identify the major cause of the gradual decrease in C2H4 FE over the operating time, we characterized the Cu catalyst after the reaction using SEM. The catalyst layer (Fig. 6b) was found to be much thinner than that for the catalysts before (Fig. 2d) or after continuous ECR tests (Fig. 2e). We reason that the Cu at the Cu/PTFE interface and at the top of the catalyst layer can migrate during the oxidation cycle i.e., when Cu is oxidized to Cu oxide. This gradual migration of Cu species over the reaction time could lead to the redistribution of Cu on the PTFE substrate, forming Cu/PTFE locations with different Cu thicknesses. In a flow cell configuration, phenomena such as catalyst fragmentation66 and agglomeration,37,67 Ostwald ripening,36,68 particle dissolution and (electro-) redeposition39 of dissolved copper species in the form of new smaller Cu fragments, as we observed in Fig. 6b, cannot be neglected. Over time, these effects could result in the formation of some areas with very thick Cu while the Cu layer may disappear in other areas, leading to the degradation of the Cu/PTFE catalyst layer when using the alternating current approach. In addition, the impact of other associated failure mechanisms resulting from the type of electrolyzer system architecture being used can lead to a systemic failure of the overall cell system. For a flow cell architecture, as we employed in this study, the additional impact of flooding and salt formation within the PTFE pores cannot be ignored for an extended testing time. These failure mechanisms, through the interdependent nature of the cell system architecture, directly impact and combine with the major failure resulting from our strategy to suppress the stability performance of the electrolyzer system and thereby limit its overall operating time.
The gaseous products were quantified using online gas chromatography (GC, PerkinElmer Clarus 590). The GC was equipped with a thermal conductivity detector (TCD) and a flame ionization detector (FID). The chromatography instrument was directly connected to the outlet of the CO2 gas chamber of the customized gas-fed flow cell for continuous online analysis. The liquid products were analyzed using nuclear magnetic resonance spectroscopy (NMR). The 1H NMR spectra of freshly collected liquid products were acquired on an Auto-400 ultrashield Bruker instrument operating at a denoted spectrometer frequency given in megahertz (MHz) at 25 °C in D2O using water suppression mode, with dimethyl sulfoxide (DMSO) as a reference.
All potential data were presented versus Ag/AgCl. However, iR-compensation was performed, and the details are presented in the supplementary section (Fig. S29 and S30†).
Footnote |
† Electronic supplementary information (ESI) available. See https://doi.org/10.1039/d2ta02709g |
This journal is © The Royal Society of Chemistry 2022 |