Bramha Guptaa,
Rushikesh S. Ambekarb,
Raphael M. Tromerc,
Partha Sarathi Ghosala,
Rupal Sinhaa,
Abhradeep Majumderd,
Partha Kumbhakarb,
P. M. Ajayane,
Douglas S. Galvao*c,
Ashok Kumar Gupta*f and
Chandra Sekhar Tiwary*b
aSchool of Water Resources, Indian Institute of Technology Kharagpur, Kharagpur 721302, India
bMetallurgical and Materials Engineering, Indian Institute of Technology Kharagpur, Kharagpur 721302, India. E-mail: chandra.tiwary@metal.iitkgp.ac.in
cApplied Physics Department, State University of Campinas – UNICAMP, 13083-859-Campinas, SP, Brazil. E-mail: galvao@ifi.unicamp.br
dSchool of Environmental Science and Engineering, Indian Institute of Technology Kharagpur, Kharagpur 721302, India
eDepartment of Materials Science and Nanoengineering, Smalley-Curl Institute, Rice University, Houston, Texas 77005, USA
fEnvironmental Engineering Division, Department of Civil Engineering, Indian Institute of Technology Kharagpur, Kharagpur 721302, India. E-mail: agupta@civil.iitkgp.ac.in
First published on 1st June 2021
The impact of micro and nanoplastic debris on our aquatic ecosystem is among the most prominent environmental challenges we face today. In addition, nanoplastics create significant concern for environmentalists because of their toxicity and difficulty in separation and removal. Here we report the development of a 3D printed moving bed water filter (M-3DPWF), which can perform as an efficient nanoplastic scavenger. The enhanced separation of the nanoplastics happens due to the creation of a charged filter material that traps the more surface charged nanoparticles selectively. Synthetic contaminated water from polycarbonate waste has been tested with the filter, and enhanced nanoplastic removal has been achieved. The proposed filtration mechanism of surface-charge based water cleaning is further validated using density function theory (semi-empirical) based simulation. The filter has also shown good structural and mechanical stability in both static and dynamic water conditions. The field suitability of the novel treatment system has also been confirmed using water from various sources, such as sea, river, and pond. Our results suggest that the newly developed water filter can be used for the removal of floating nanoparticles in water as a robust advanced treatment system.
Advanced physical treatment processes, such as dissolved air floatation, rapid sand filter, disc filters, and biological processes, have been employed to remove microplastics from the wastewater.17–21 The average removal efficiency using disc filters was found to be around 40%, while dissolved air floatation and rapid sand filtration techniques accounted for removal of around 48% and 90%, respectively.17 Filtration is considered an effective technique for the removal of microplastics due to its trapping and adsorption ability. On the other hand, for separation of nanoplastics using the conventional filters have several limitations, such as low filtration efficiency, poor mechanical resistance, and pore blockage.22 The filtration efficiency is improved with the help of increasing surface area of the porous architecture.23 The porous filters are fabricated by gas foaming, solvent casting/particulate leaching, freeze-drying, and 3D printing24–29 techniques. Among these, 3D printing is the competitive technique due to its numerous advantages, such as its capability to fabricate complex structures, agility to print a wide spectrum of compatible materials, sustainability, and scalability.30–36 Furthermore, a schwarzite-based 3D structured porous filter was used due to its large surface area, positive and negative curving topologies with tunable spongy size and shape, and intriguing properties. These crystalline constructions can have a large number of porous unit cells, rigid foam-like materials with tunable mechanical and electronic properties.27,37
The separation of nanosized particles is more difficult compared to the higher-sized particles in the conventional filtration process, which creates significant difficulties in nanoplastics removal from an aqueous solution. We determined that the selectivity towards nanosized particles for a charged filter media can be developed from the fact that the surface charge of the particles increases with the decreasing particle size, which can be due to the surface area effect.38,39 Thus, the development of a novel nanoplastics removal system can be exploited from this innovative separation concept.
In this study, we have fabricated a novel 3D printed moving bed water filter (M-3DPWF) targeting the filtration of nanoplastics (as shown in Fig. 1). The structural ability of the M-3DPWF was tested by measuring its compressive stress, yield stress, and toughness (as depicted in Fig. 2). The M-3DPWF was employed to treat polycarbonate contaminated synthetic water. Microscopy and spectroscopy of the M-3DPWF treated water were also carried out to confirm the nanoplastics removal. The field suitability of the M-3DPWF was further tested using source water from the sea, river, and pond. The proposed mechanism of surface charge-based water cleaning is further supported using DFT-based simulation. The proposed technology can be an advanced and feasible solution for the concerns of nanoplastics contamination in water bodies worldwide.
Fig. 1 Scheme of the M-3DPWF preparation, its use for nanoplastics filtration, physicochemical assessment of the filtration performance, and filtration mechanism. Scale bar 500 nm. |
The presence of nanoplastics in the water samples was assessed by measuring its particle size distribution in water before and after treatment conditions. Particle concentration in the treated water was measured using a Zetasizer, which corresponds to the removal of nanoplastics. Spectroscopic and microscopic analyses of the contaminated water at both the initial and final stages were also performed to get the physicochemical attributes of the nanoplastics. The Fourier transform infrared (FTIR) analysis of the source, raw, and treated water was carried out using FTIR spectroscopy (Nicolet-6700, Thermo Fisher, USA), having wavenumbers ranging from 250 to 4250 cm−1. The surface morphology was assessed by field-emission scanning electron microscopy (FE-SEM) analysis (ZEISS-MERLIN, GEMINI-2, Germany). The sample preparation procedures for FTIR and FE-SEM analysis have been given in ESI (Section S1†). High-resolution transmission electron microscopy (HR-TEM) was carried out to obtain the in-depth surface morphology and size distribution at the nanoscopic level (JEM-2100F, Make-JEOL, Japan). Thermogravimetric analysis (TGA) was performed using a thermogravimetric/differential thermal analyzer (Perkin Elmer Pyris Diamond TG/DTA, USA) by introducing nitrogen gas and increasing temperature at 10 °C min−1. Zeta potential and average particle size of the treated water were measured using a Zetasizer Nano ZS90 analyzer (Malvern, UK).
E = EAB − EA − EB | (1) |
The M-3DPWF was used to treat nanosized polycarbonate polluted water. The spectroscopy and microscopy analyses of the treated water were carried out to obtain the filtration performance of the 3D printed water filter. In Fig. 3a, the schematic shows the preparation process of polycarbonate nanoparticles. The FTIR spectra (Fig. S1a, d, and e, ESI†) of the initial and treated water show the presence of the chemical bonds of the polycarbonate plastics in the solution, as discussed in the ESI (Section S2).† There is no peak shift in the FTIR spectra of the initial and final solution, which confirms that there is no change in the chemical behavior of polycarbonate during the removal process. In Fig. 3b and d we present the FE-SEM images of the initial and treated water. The low magnification SEM image of the polluted water shows a large number of flake-like polycarbonate particles (Fig. 3b). The microscopic size analysis of polluted water [as shown in histogram (inset of Fig. 3b)] reveals the particles were in the size range of 1000–9000 nm, with the majority of the particles being below 3000 nm. The HRTEM analysis of polluted water (Fig. 3c) shows the presence of 25–160 nm-sized polycarbonate particles with most particles being below 70 nm [as shown in histogram (inset of Fig. 3c)]. The FE-SEM of treated water (Fig. 3d) shows a drastic reduction in the number of observed particles (1000–9000 nm). The few particles observed in the micrograph are of 9000–10000 nm size range [as shown in the inset of Fig. 3d)]. The HRTEM of treated water has also shown a drastic decrease in the number of observed particles (25–160 nm) (Fig. 3e). Even in the histogram of treated water (inset of Fig. 3e), it can be seen that particles up to size 60 nm are absent. These results confirm that the M-3DPWF is efficient to remove nano (majorly) and micro-size polycarbonate particles from the water. The Zetasizer analysis (Fig. 3f) shows that the frequency of particle size distribution predominantly varies in the range of 70–105 nm, wherein around 90 nm sized particles occur most frequently in the polluted water. On the other hand, the frequency distribution of particles present in the treated water was shifted to a higher range (90–125 nm) with the maximum occurring particles of size ∼110 nm. The bar diagram of treated water exhibited the drastic reduction of smaller size polycarbonate particles, which is ascribed to the filtration ability of the M-3DPWF in the removal of the nanosized polycarbonate plastics (Fig. 3f). Additionally, from Fig. S2,† it can be seen that in raw water the maximum number of particles (about 50%) is of size about 190 nm (Fig. S2a†), while in treated water the maximum number of particles (about 40%) are of size more than 400 nm (Fig. S2b†), which confirms the separation of polycarbonate nanoparticles using the M-3DPWF. Furthermore, from Fig. S3,† it can be observed that the distribution of the particles in the different samples of polycarbonate for initial and treated water are varying. For example, for treated water, the sample was collected from the top, middle, and bottom locations, which is showing the average particle size of, ∼30 nm, ∼51 nm, and ∼106 nm, respectively. Whereas, for three initial samples, it was ∼87 nm, ∼91 nm, and ∼165 nm, respectively.
The removal of polycarbonate particles from the polluted water was further validated using UV absorbance data, as shown in Fig. 3g. The absorbance of the treated water is lesser than the nanoplastics polluted water. The presence of more nanoparticles in the polluted water will block the path of UV light, which is responsible for its higher absorbance. The reduced absorbance of the treated water is attributed to the filtration ability of the M-3DPWF for the removal of polycarbonate particles (nano and micro). To test the maximum filtration ability of the 3D water filter, filtration of polycarbonate polluted water was further performed above 48 h. From Fig. S4,† it is observed that the absorbance of the treated water did not significantly change at 60 h, hence it can be concluded that the 3D water filter is showing the maximum filtration ability at 48 h. From the zeta potential plot (Fig. 3h), it can be observed that the zeta potential is lower for the treated solution (∼−3.0 mV) than the initial solution (∼−6.5 mV). The decrease in the zeta potential can be attributed to the removal of charged polycarbonate (small-sized) particles through filtration.
The presence of plastics (micro and nano) in the different source water, such as sea, river, and pond were assessed by performing spectroscopic and microscopic analyses. The source water was collected from the Bay of Bengal (Digha, East Midnapore, West Bengal, 21°37′35.8212′′N 87°30′26.7516′′E), Hooghly River (Konnagar, Hooghly, West Bengal, 22°42′18.3′′N 88°20′40.1′′E), and Black Lake (IIT Kharagpur, Kharagpur, West Midnapore, West Bengal, 22°19′6.58′′N 87°18′21.52′′E), respectively. The collected water was preserved, and subsequently, its physicochemical analysis was carried out. The images of source water (sea, river, and pond) are shown in Fig. 4a–c. The FTIR spectra of the source water (Fig. S1b, c, and f, ESI†) have shown the presence of polyethylene, polypropylene, polyvinyl chloride, nylon-6, polystyrene, and polycarbonate, as discussed in the ESI (Section S1).†
The FE-SEM analysis (Fig. 4d, f, and h), revealed that sea, river, and pond water samples contain flakes and granular-like particles. The presence of dark patches in the FE-SEM images may belong to organic solids in water. The histogram of the micrograph (Fig. S5a–c†) displays the presence of maximum particles up to the size of 10000, 40000, and 100000 nm for sea, river, and pond water, respectively. The HRTEM analysis of source water (sea, river, and pond) has shown the presence of plastic particles (bright particles) along with other organic solids (Fig. 4e, g, and i). Further, the histogram of HRTEM analysis (Fig. S5d–f†) shows that most particles are found up to size 70, 30, and 8 nm for sea, river, and pond water, respectively. These results confirm that the seawater contains nanoparticles in a larger size range (∼70 nm) and microparticles in a smaller size range (∼10000 nm) than those in river and pond water. The zeta size analysis shows that the average size of the particles in the sea, river, and pond water is 73.82, 217.1, and 155.6 nm, respectively, as shown in Fig. 4j, which confirms that the nanoparticles are more in numbers in the initial sample. These results confirm that the frequency of larger size particles in the river and pond water is higher than the seawater. The UV absorbance of the source water was measured and shown in Fig. 4k. This result shows that the absorbance of the source water follows the order like sea > river > pond, which confirms that the seawater contains smaller size particles than the river and pond water. From TGA, it was observed that solids from the pond showed more weight loss (∼22%) than sea and river water solids (∼15% and ∼10%, respectively) over a temperature range of 40–600 °C (Fig. 4l). In this case (for 40–600 °C), weight loss is directly related to the organic content, and it can be inferred that pond water contains more organic solids or lesser plastic contents.50 The organic solids having more plastic content will show high thermal stabilities due to the high thermal resistance of the plastics. Apart from that, the plastics will act as media to carry the hydrophobic organic carbons as suggested by Koelmans et al. (2016).51 From FTIR analysis, it has been found that the source waters contain plastics, so the thermal stabilities of its solids will get increased. Çepelioǧullar, Ö. & Pütün et al. reported that the presence of plastics such as polyethylene terephthalate and polyvinyl chloride had increased the thermal stability of the biomass,52 which is similar to the present study. Hence, the solids from sea and river water, which showed increased thermal stabilities may correspond to the presence of more plastic (nano and micro) particles along with other organics.
The real-life field samples from sea, river, and pond were treated by the M-3DPWF system. The physicochemical characterization of the treated water was conducted by zeta size analyzer and UV-vis absorbance measurement. The zeta size analysis of the treated water was performed and is shown in Fig. 4j. Particle size analysis has shown that the average size of the particles in the sea, river, and pond water is 165.1, 372.5, and 510.8 nm, respectively, which confirms that most of the particles are of micro size. The drastic increment in the average size of the particles in all the treated water samples can be attributed to an increased removal of nanosized compared to the micro-sized particles. Furthermore, the UV-vis absorbance (Fig. 4k) of the treated water shows a drastic reduction, which confirms the removal of plastics during the treatment process. Thus, M-3DPWF based treatment system can be successfully employed for field-based real-life water of various sources such as sea, river, and pond.
Generally, the plastics suspended in the polluted water have a surface charge. In order to attract/adhere to the charged particles, we can print the 3D block using oppositely charged materials. In order to have further insights about these aspects at the atomic scale, we carried out semi-empirical quantum simulations using ABS and PC model chains (see Fig. 5I–IV) to understand the removal mechanism concerning the role of surface charge.
As discussed in the materials and methods section, we used PM7 to obtain the optimized geometries, configuration energy (eqn (1)), and charges (electrostatic maps). We tested for other similar parameterizations available in the MOPAC2016, such as PM6 and PM6-DH2, but the results were almost the same. We also tested the solvent effect considering the COSMO method implemented in the MOPAC2016,53 assuming that water is modeled as a dielectric medium with a K (dielectric constant) equal to 78.4. We verified that the solvent does not significantly affect the total energy values. Fig. 5II–V shows the interaction energy values as a function of separation R between ABS and PC molecules. We considered four configurations of the ABS molecule placed at the origin of the axis (Fig. 5II, III and S6†). For each ABS configuration, we consider four different PC configurations. As we can see from Fig. 5II, III and S6† there are not very significant energy variations for the different configurations unless the molecules come very close. In Table 1, we present the heat of formation values for the optimized configurations, considering the ABS as located at the origin reference. In this case, there are energy variations but in the range window of less than 5 kcal mol−1. These results show that depending on the configuration, there is a strong ABS/PC interaction. These aspects can be better understood by analyzing the charge transfer and the electrostatic maps of the different configurations. In Table 2, we present the charge profile for the optimized structures from Table 1. The minus sign corresponds to the transferred charge to ABS. Although the specific charge transfer values depend on the configuration (positive and negative), the observed general trend is that the ABS becomes negative. In Fig. 5IV, we present some examples of the electrostatic maps. For these configurations, the transferred charge between ABS and PC was (in me units): −1.36, −4.20, −4.69, and −3.45, respectively. Molar attraction constant is the ability of individual molecules/functional groups to attract another molecule due to intermolecular forces such as dipole–dipole interaction, π–π interaction, and H-bonding. The minus sign means the charge is transferred to ABS. Further, ABS (base material of the M-3DPWF) and PC have higher molar attraction constant (∼1943 and ∼2384 J1/2 cm3/2 mol−1, respectively), which will cause electrostatic attraction among them.28
conf1 | conf2 | conf3 | conf4 | |
---|---|---|---|---|
ABS1 | −3.00 | −2.00 | −2.9 | −4.72 |
ABS2 | −4.89 | −1.52 | −1.74 | −2.45 |
ABS3 | −0.40 | −1.24 | −1.40 | −3.64 |
ABS4 | −2.65 | −4.29 | −2.77 | −2.78 |
conf1 | conf2 | conf3 | conf4 | |
---|---|---|---|---|
ABS1 | −1.25 | 1.30 | 0.79 | −1.36 |
ABS2 | −0.02 | −2.98 | 0.03 | −4.20 |
ABS3 | −2.31 | −0.35 | −4.69 | −0.94 |
ABS4 | 1.22 | −6.24 | −3.25 | −3.45 |
The present separation mechanism for the nanoplastics is designed utilizing the electrostatic attraction of the filter material and the charged particles. The size exclusion mechanism depends on the quantity of the surface charge of the suspended particles. We should stress that the DFT calculations used here do not intend to simulate the whole filter process. Even models based on large molecular dynamics simulations cannot incorporate all details of the filter process to be investigated. The DFT simulations were used as a proof of concept and to obtain further insights on specific aspects of the charging behavior due to electrostatic effects caused by the interaction between two prototypes, ABS (base material of the M-3DPWF) and polycarbonate, both present in the filter process. This issue has been hotly debated in the literature sometimes with conflicting results. In order to obtain some insights into the triboelectric effects used on the filter separation process, we recalculated the charge transfer but added one electron (charge = −1e) to the system. In this case, the minus sign means the electron excess. We can see from Table 3 that in all cases the tendency is the extra electron to be localized in one of two molecules and of the order of one electron. Thus, we can assume that one of the species remains charged with one electron excess. This observation gives us insights into the possibility of ABS and polycarbonate be used in the filter process through triboelectric separation effects. Thus, the M-3DPWF treatment system can be considered to be a robust process for the removal of nanoplastics by an innovative separation technology.
1 | 2 | 3 | 4 | ||
---|---|---|---|---|---|
conf1 | (ABS/polycarbonate) | (−0.99e/−0.01me) | (−2.9me/−1.0e) | (−10.0me/−0.99e) | (−15.4me/0.99e) |
conf2 | (ABS/polycarbonate) | (−17.2me/−0.98e) | (−21.3me/−0.98e) | (−0.98e/−17.2me) | (−11.7me/0.99e) |
conf3 | (ABS/polycarbonate) | (−6.51me/−0.99e) | (−6.45me/−0.99e) | (−2.6me/−1.0e) | (−8.9me/0.99e) |
conf4 | (ABS/polycarbonate) | (−20.4me/−0.98e) | (−9.3me/−0.99e) | (−10.7me/−0.99e) | (−18.0me/0.98e) |
We carried out fully-atomistic molecular dynamics (MD) simulations with the reactive force field ReaxFF potential,54 as implemented in the Large-scale Atomic/Molecular Massively Parallel Simulator (LAMMPS).55 We used the parameters set provided by Chenoweth et al. for C/H/N/O.56 We adopted an NVT ensemble and Nosé–Hoover thermostat.57 The equations of motion were numerically integrated using the velocity-Verlet integrator with a time-step of 0.1 fs for a total simulation time of 100 ps.
In order to represent the ABS membrane, we considered that the molecules were pre-optimized at the DFT level. We built the membrane considering the alignment of the molecules along the x-direction, in which the membrane is periodic in the xy-plane. We considered also cases where the membrane is not infinity (cyclic boundary conditions) along the y-direction, see Fig. S7 in the ESI.† The smallest thickness of the ABS membrane is about 4 Å. The separation between the ABS membranes corresponds to 60 Å (Fig. S8 in the ESI†). We performed several simulations for different membranes (types, thickness, and periodic conditions).
Fig. S9† shows representative MD snapshots of the initial configuration at t = 0 ps (at left) and the last step corresponding to 100 ps (at right). In Table S2 of the ESI,† we present the relevant parameters for each simulation. We also included the video containing the trajectories for simulations (c), (d), and (f). Simulation of ABS membrane with larger thickness membrane is shown in the Video SV1.† For membranes with the smaller thickness, we observed that ABS molecules are stacked resulting in membrane contraction, as in the MD simulation shown in the Video SV2.† We observed in the last snapshot of all cases the cluster formation with different sizes because of the interaction between the polycarbonates and water molecules. This is in agreement with the experimental data where the particle sizes varying from 1000 to 9000 nm. In all cases, we observed a significant tendency of occurring an attraction between ABS membranes and the polycarbonate plus water clusters. I should be stressed that in all cases the majority of the clusters is attracted to the ABS membrane. This corroborates our interpretation of the results discussed in this manuscript where we analyzed the interaction energy between ABS and polycarbonate. Therefore these results further validate the experimental conclusions that ABS membranes can be a good plastic absorber in an aqueous environment.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra03097c |
This journal is © The Royal Society of Chemistry 2021 |