aChemical Engineering Group, Engineering and Technology Institute Groningen (ENTEG), University of Groningen, Nijenborgh 4, 9747 AG Groningen, The Netherlands. E-mail: p.p.pescarmona@rug.nl
bZernike Institute for Advanced Materials, University of Groningen, Nijenborgh 4, 9747 AG, Groningen, The Netherlands
First published on 4th July 2019
Multifunctional catalytic systems consisting of physical mixtures of (i) bimetallic Au–Pd nanoparticles (average size of 3–5 nm) supported on functionalised carbon nanotubes (CNTs) and (ii) Sn-MCM-41 nanoparticles (50–120 nm), were synthesised and investigated for the base-free, selective conversion of glycerol to methyl lactate in a batch reactor. The catalysts were characterised by means of transmission electron microscopy, N2-physisorption, energy-dispersive X-ray spectroscopy, X-ray photoelectron spectroscopy and by Boehm titration. The catalyst based on bimetallic AuPd/CNTs showed much higher activity than the monometallic Au or Pd counterparts, thus indicating synergetic effects. Functionalisation of the CNTs by oxidative treatments had a positive effect on catalyst performance, which was correlated to the observed increase in surface acidity and hydrophilicity. The highest yield of methyl lactate achieved in this work was 85% at 96% glycerol conversion (140 °C, 10 h at 30 bar air), which is the highest yield ever reported in the literature so far. Insights in the reaction pathway were obtained by monitoring the conversion-time profiles for intermediates and their possible role as inhibitors. Batch recycling experiments demonstrated the excellent reusability of the catalyst.
Scheme 1 Catalytic route from glycerol to methyl lactate (ML) and, in grey, the possible side-products. |
In order to promote the cascade reaction in Scheme 1 in a base-free reaction medium, two kinds of catalytic species are needed: (i) (supported) noble metal nanoparticles (NPs) for the partial oxidation of glycerol; (ii) a solid acid catalyst with Lewis and Brønsted acid sites for the rearrangement step.13,14,20,21 Here, we report for the first time the use of bimetallic Au–Pd nanoparticles supported on (functionalised) carbon nanotubes as catalysts for the oxidation step of glycerol to glyceraldehyde or dihydroxyacetone. Previous work demonstrated that this first step of the reaction is the one on which research should be mainly focussed to increase the overall activity and selectivity of the catalytic system.15 Therefore, we focussed our efforts on designing an enhanced catalyst for this initial step, while employing the optimum solid acid catalyst identified in previous work (i.e. Sn-MCM-41-XS)15,20,22 for promoting the rearrangement of trioses into lactates. We reasoned that the catalyst for the partial oxidation of glycerol could be improved by employing bimetallic nanoparticles, as the presence of a second metal can allow tuning the electronic properties, morphology and stability of the nanoparticles towards increased activity and selectivity.23,24 Therefore, we chose to combine Au with another, relatively less expensive noble metal, Pd, which has proven to lead to increased catalytic performance when used in an alloy with Au in several partial oxidation reactions.3,8,23–28 A second factor that plays an important role for the catalytic behaviour of (bi)metallic nanoparticles is the nature of the support.29,30 In this work, functionalised multi-walled carbon nanotubes (CNTs) were selected as support for the bimetallic nanoparticles. Carbon nanotubes display a large, accessible external surface area and high chemical and thermal stability, which make them attractive supports for metal nanoparticles.31–34 Additionally, carbon nanotubes can be modified by oxidative methods to tune their surface properties like acidity, hydrophilicity and dispersibility.30,35–37 Such functionalisation of the CNTs surfaces was shown to have a positive effect on catalyst performance due to enhanced interactions between the metallic nanoparticles as well as with the substrates.30–32,38,39 However, there is no report in the literature on the use of mono- or bimetallic Au-based nanoparticles supported on functionalised CNTs for the base-free glycerol oxidation to lactic acid/alkyl lactates. Based on these considerations, our strategy involved the synthesis, characterisation and testing of multifunctional heterogeneous catalytic systems for the conversion of glycerol to methyl lactate, consisting of physical mixtures of (i) bimetallic Au–Pd nanoparticles supported on different functionalised CNTs and (ii) Sn-MCM-41-XS. The performance of the bimetallic nanoparticles was compared to the monometallic (Au or Pd) counterparts. The choice of using a physical mixture of the supported nanoparticles and Sn-MCM-41-XS rather than supporting the metal nanoparticles directly on Sn-MCM-41-XS was based on the previously observed infeasibility of achieving high loading of well dispersed nanoparticles without causing the deterioration of this mesoporous material.15 In addition, the use of two materials allows higher flexibility in terms of adjustment of the Sn to noble metal ratios. The batch reactions were carried out in methanol (which has been identified as a “recommended” solvent in the context of green chemistry40) without the addition of an external base and using air as the oxidant at relatively mild conditions for this reaction (see Table S1†).
Entry | Catalyst | Au + Pd loading (wt%) | Molar ratio of Au/Pd | |
---|---|---|---|---|
Theoretical | Experimental | |||
1 | Au/CNTs | 1.2 | — | — |
2 | Au3Pd/CNTs | 1.0 | 3 | 3.1 |
3 | AuPd/CNTs | 1.0 | 1 | 1.2 |
4 | AuPd3/CNTs | 1.0 | 0.33 | 0.4 |
5 | Pd/CNTs | 0.9 | — | — |
Entry | Sample | Specific surface areaa (m2 g−1) | Pore volumeb (cm3 g−1) | C atomic%c | O atomic%c | S atomic%c | Total acid sitesd (mmol g−1) | Stronger acid sitesd (mmol g−1) |
---|---|---|---|---|---|---|---|---|
a BET surface area. b BJH cumulative volume of pores, between 17 and 3000 Å width, based on the desorption isotherm. c C, O, S atomic content (mol%), as determined by EDX. d The amount of total and stronger acid sites was determined by Boehm titration of NaOH and NaHCO3, respectively. CNTs-O, CNTs-N, CNTs-S, CNTs-NS denote the CNTs treated by H2O2, HNO3, H2SO4 and H2SO4–HNO3, respectively. n.d. = not determined. | ||||||||
1 | CNTs | 258 | 2.1 | 99.2 | 0.8 | — | 0.022 | 0.002 |
2 | CNTs-O | 313 | 2.0 | 98.7 | 1.3 | — | 0.90 | 0.42 |
3 | CNTs-N | 306 | 2.0 | 98.5 | 1.5 | — | 1.3 | 0.88 |
4 | CNTs-S | 259 | 2.1 | 98.8 | 1.1 | 0.11 | 0.46 | 0.23 |
5 | CNTs-NS | 274 | 1.6 | 97.3 | 2.6 | 0.10 | 2.4 | 1.3 |
6 | AuPd/CNTs | 241 | 2.0 | n.d. | n.d. | n.d. | n.d. | n.d. |
TEM images of the bimetallic catalysts demonstrate the successful synthesis of metal nanoparticles with an average size of around 6 nm and a relatively broad particle size distribution from 1 to 16 nm (Fig. 1A). The relatively larger nanoparticles consist of aggregated and partially coalesced smaller nanoparticles. This is probably due to the weak interaction between the CNTs surface and the nanoparticles during the colloid immobilisation process. As a reference, bimetallic Au–Pd nanoparticles supported on unmodified activated carbon (AC) using the same synthesis protocol also showed (Fig. 1B) coalesced nanoparticles with a large average size (9.9 nm) and a large particle size distribution (1–24 nm), thus supporting the hypothesis that unfunctionalised carbon surfaces tend to lead to relatively large nanoparticles.
Fig. 1 TEM pictures of bimetallic Au–Pd nanoparticles supported on unmodified CNTs and AC. A: AuPd/CNTs, average size = 6.0 nm; B: AuPd/AC, average size = 9.9 nm. |
The monometallic Au/CNTs, Pd/CNTs and bimetallic AuPd/CNTs catalysts were characterised by XPS to determine the surface composition and, in the case of the bimetallic catalyst, to investigate whether the metals are actually forming an alloy, or are present as isolated Au and Pd nanoparticles, or as a combination of the two. Based on thermodynamic considerations, the formation of an Au–Pd alloy is expected to be favoured as negative enthalpies of formation have been observed for the Au–Pd system.41 XPS confirms the presence of the metals employed in the synthesis in all samples (Au/CNTs, Pd/CNTs and AuPd/CNTs, Fig. 2). The analysis of the chemical states of Au and Pd was based on the Au 4f7/2 and Pd 3d3/2 signals, which are devoid of the overlap observed between Au 4d5/2 and Pd 3d5/2 or between Au 4f5/2 and Pd 4s.42,43 The Au 4f7/2 peak was found at 84.2 eV in the monometallic Au/CNTs catalyst (Fig. 2a), while it was shifted by about 0.5 eV towards lower binding energy in the bimetallic AuPd/CNTs (Fig. 2b). The same trend was found for the Pd 3d3/2 peak, which was shifted by 0.8 eV towards lower binding energy in the bimetallic AuPd/CNTs sample (Fig. 2d) compared to the monometallic Pd/CNTs one (Fig. 2c). The observed decrease in binding energy of both Au 4f7/2 and Pd 3d3/2 compared to the monometallic counterparts is in line with what has been previously observed in other Au–Pd systems and has been attributed to the formation of an Au–Pd alloy.44,45
Fig. 2 XPS signals of the Au 4f core level region for (a) Au/CNTs, (b) AuPd/CNTs, and of the Pd 3d core level region for (c) Pd/CNTs, (d) AuPd/CNTs. |
XRD analysis of the AuPd/CNT materials (Fig. 3) confirmed the formation of the Au–Pd alloy. After loading the Au–Pd nanoparticles on the CNTs, only one new, broad peak (due to the small size of the particles) appears in the XRD pattern at 39.36°. Its position is in between that of the (111) peak of monometallic Au (38.27°) and of the (111) peak of monometallic Pd (40.42°), in agreement with the formation of an Au–Pd alloy.
The two monometallic and the bimetallic Au–Pd catalysts on unmodified CNTs were investigated for the conversion of glycerol into methyl lactate in combination with Sn-MCM-41-XS in a batch set-up (140 °C, 30 bar air pressure, Fig. 4). The monometallic Au/CNTs catalyst showed 25% conversion of glycerol and 93% selectivity towards methyl lactate. By gradually increasing the relative Pd content of the catalyst (nominal Au/Pd molar ratio of 3/1; 1; and 1/3), the conversion first increased from 41% to 47% and then decreased to 41% (Fig. 4). The conversion further decreased to 35% when the monometallic Pd/CNTs was used. Conversely, the selectivity towards methyl lactate remained nearly constant at around 90% regardless of the Au/Pd molar ratio.46 The role of the (bi)metallic nanoparticles is to catalyse the first step of glycerol oxidation (i.e. the initial activation of oxygen and/or glycerol, step A in Scheme 1).15,20 The optimum synergistic effect was found for a nominal Au/Pd molar ratio of 1 (actual ratio = 1.2, see Table 1), which matches our anticipation that alloying Au with Pd would lead to enhanced activity. This trend is in agreement with the increase in the rate of the oxidation of alcohol groups of other organic compounds (e.g. benzyl alcohol and 5-hydroxymethylfurfural) that was observed by using bimetallic Au–Pd instead of monometallic Au catalysts.30,47
Elemental analysis of the CNTs by EDX allowed determining the C, O and S content at the surface, which provides information on the degree of functionalisation of the CNTs. In the untreated CNTs, the oxygen amount is only 0.8%, whereas all the treatments largely enhanced the oxygen content of the CNTs. The highest value (2.6%, entry 5, Table 2) was obtained upon treatment with a H2SO4–HNO3 mixture. The increased O content indicates the formation of considerable amounts of oxygenated groups (e.g. –OH, –CHO, –COOH) on the surface of the CNTs.48,49 The presence of such oxygenated groups leads to a higher surface acidity, but also significantly improves the hydrophilicity of the CNTs surface. Both features can be important for the catalytic performance of the supported (bi)metallic nanoparticles. The higher surface acidity can promote the acid-catalysed dehydration step of the conversion of glycerol into methyl lactate (i.e. step B in Scheme 1). The higher hydrophilicity can: (i) enhance the interaction with the nanoparticles during their preparation by colloidal immobilisation; (ii) affect the reaction rates by changing the adsorption constants of substrates and products on the surface; (iii) promote the dispersion of the CNTs in a polar reaction medium (which is an asset both for the preparation of the supported nanoparticles as well as for the catalytic reaction). The treatment of CNTs with H2SO4 (entries 4 and 5) is known to lead to the formation of sulphonic acid groups (–SO3H) on the CNTs surface, which is confirmed by the presence of significant amounts of sulphur in these materials (0.1%, see Table 2). The number and strength of the acid sites of the functionalised CNTs were evaluated by Boehm titration with an aqueous solution of NaOH, for the total number of acid sites, and with an aqueous solution of NaHCO3 for the determination of the stronger acid sites (i.e. carboxylic and sulphonic groups).50,51 The untreated CNTs material has a low amount of acid sites (0.022 mmol g−1 in total, entry 1, Table 2). All treatments resulted in an increase in total acid sites. The highest values in the concentration of both strong (1.3 mmol g−1) and total (2.4 mmol g−1) acid sites were obtained upon treatment of the CNTs with H2SO4–HNO3. The total amount of acid sites correlates well with the oxygen content after treatment, Fig. S1.†49 The anticipated effect of the functionalisation of the carbon nanotubes on their ability to form a stable dispersion in a polar medium was estimated by sonicating the CNTs for 1 h in water, followed by storage without agitation. After one week in static conditions, the parent CNTs and CNTs-S had separated at the bottom of the vial, whereas the CNTs treated by H2O2, HNO3 and H2SO4–HNO3 (i.e. those with the highest degree of functionalisation, see Table 2) were still dispersed in the water phase (Fig. S2†). Placing a droplet of each of these suspensions on a filter paper indicated a different degree of aggregation of each type of functionalised CNTs (Fig. S2†). Particularly, the larger, uniform, dark grey spot generated by CNTs-NS showed that this material has the highest tendency to from a homogenous dispersion in water. This result correlates well with the higher oxygen content and total acid amount of these functionalised CNTs, which cause the material to be more hydrophilic.29 The partial cleavage of CNTs into smaller fragments that has been reported to be caused by the harsh treatment with H2SO4–HNO3 probably also contributes to the enhanced dispersibility of CNTs-NS.48,52
The functionalised CNTs were used as support for a range of bimetallic Au–Pd catalysts prepared using a similar CI method to the one employed with unmodified CNTs (vide supra). As anticipated, the functionalisation method had a large effect on the average size of the Au–Pd NPs on the support,48,52 as evidenced by TEM analysis (Fig. 5). The average particle size and size distribution show a correlation with the degree of functionalisation of the CNTs surface,41,45 with the Au–Pd nanoparticles supported on CNTs prepared in the presence of HNO3 (CNTs-N and CNTs-NS, i.e. those with the highest concentration of functional groups, see Table 2) having the smallest average size (∼3.5 nm), with a narrow particle size distribution. The smaller average size of the Au–Pd nanoparticles observed by TEM in AuPd/CNTs-NS (3.5 nm, Fig. 5D) compared to those in AuPd/CNTs (6.0 nm, Fig. 1A) correlates well with the less intense and broader peak of the Au–Pd alloy observed in the XRD pattern of the former material (Fig. 3).
The bimetallic Au–Pd nanoparticles supported on functionalised CNTs were investigated in combination with Sn-MCM-41-XS as heterogeneous catalytic system for the oxidative conversion of glycerol into methyl lactate (Table 3). We expected these catalytic systems to be superior to the counterpart based on Au–Pd nanoparticles supported on the unfunctionalised CNTs because: (i) the well-dispersed Au–Pd nanoparticles have smaller average size, (ii) the functionalised CNTs disperse better in the polar reaction medium and (iii) provide additional surface Brønsted acid sites for promoting the dehydration step from trioses to pyruvic aldehyde.13,15,20 Indeed, the rate of glycerol conversion was higher with the functionalised CNTs, the only exception being the CNTs treated with H2O2, which performed as the untreated CNTs (Table 3, entries 1 to 5). The impact of the nature of the support on the performance of the catalytic system was highlighted by the dramatic increase in the conversion of glycerol passing from the untreated CNTs (54% conversion) to the CNTs that underwent the treatment with HNO3–H2SO4 and which display the largest concentration of acid groups, including strong sulphonic groups (81% conversion with 70% yield of ML). With prolonged reaction time (9 h), the yield of methyl lactate reached 85% at 96% glycerol conversion (Table 3, entry 6), which to the best of our knowledge is the highest yield ever reported for the conversion of glycerol to methyl lactate using a heterogeneous catalytic system (Table S1†). The main by-products identified by gas chromatography (GC) were methyl pyruvate (MP), methyl glycolate (MGo), dimethyl oxalate (DMO), dimethyl tartronate (DMT) and methyl glycerate (MGe), see Scheme 1. Carbon balances for all runs exceeded 98%, indicating that the formation of products that would not be detected by GC (e.g. higher molecular weight components formed by condensation reactions) is negligible.
Entry | Catalyst | Conv. (%) | Y of ML (%) | Selectivity (%) | |||||
---|---|---|---|---|---|---|---|---|---|
ML | MP | MGo | DMO | DMT | MGe | ||||
a Reaction conditions: 0.25 M glycerol in 20 ml methanol; 0.1 g of AuPd/CNTs; 0.2 g of Sn-MCM-41-XS; 140 °C; 30 bar air; 4.5 h. For all reactions, small amounts of pyruvic aldehyde dimethyl acetal were observed, with selectivity below 0.1%. b Reaction time: 9 h at 140 °C (heating time 0.5 h). c Run without Sn-MCM-41-XS. | |||||||||
1 | AuPd/CNTs + Sn-MCM-41-XS | 54 | 47 | 90 | 1.5 | 2.2 | 0.4 | 0.8 | 4.9 |
2 | AuPd/CNTs-O + Sn-MCM-41-XS | 54 | 46 | 88 | 2.3 | 3.0 | 0.6 | 0.6 | 5.0 |
3 | AuPd/CNTs-N + Sn-MCM-41-XS | 63 | 54 | 88 | 2.5 | 3.4 | 0.5 | 0.9 | 4.4 |
4 | AuPd/CNTs-S + Sn-MCM-41-XS | 71 | 61 | 87 | 1.9 | 1.8 | 0.4 | 1.3 | 7.2 |
5 | AuPd/CNTs-NS + Sn-MCM-41-XS | 81 | 70 | 87 | 5.6 | 1.6 | 0.2 | 0.3 | 5.1 |
6 | AuPd/CNTs-NS + Sn-MCM-41-XSb | 96 | 85 | 88 | 2.7 | 3.5 | 0.6 | 0.6 | 3.2 |
7 | AuPd/AC + Sn-MCM-41-XS | 9.3 | 7.5 | 94 | 0.4 | 1.6 | 0.5 | 0.8 | 2.8 |
8 | AuPd/CNTsc | 6.8 | 0.4 | 5.7 | 2.1 | 13 | 5.1 | 1.6 | 17 |
The decrease of the Au–Pd particle size when using the unfunctionalised carbon nanotubes as support, which implies that a higher fraction of metal sites is exposed on the surface and thus available as catalytic sites, is most likely the main factor that led to the dramatic increase in activity (from 54% with AuPd/CNTs to 81% with AuPd/CNTs-NS, see Table 3). However, the acidity of the functionalised CNTs also contributed to the observed increase in catalytic activity. This is demonstrated by the higher activity achieved with AuPd/CNTs-S compared to Au–Pd/CNTs (71% vs. 54%): both have similar particle size (∼6 nm), but the former has a large population of acid sites (Table 2). Additionally, the strength of these acid sites also plays a role: AuPd/CNTs-S has a larger particle size and lower amount of acid sites (0.46 mmol g−1) compared to AuPd/CNTs-N (particle size 3.3 nm, acid amount 1.29 mmol g−1) but showed higher activity (71% vs. 63%). This is most likely due to the presence in AuPd/CNTs-S of the sulphonic groups generated by the treatment with H2SO4, as indicated by the presence of sulphur in this material (Table 2). Though both sulphonic and carboxyl groups are labelled as strong acids on the basis of Boehm titration, the sulphonic groups are much stronger acid sites compared to the carbon-based acid groups in AuPd/CNTs-N and, therefore, promote more efficiently the dehydration step of trioses to pyruvic aldehyde.53 A similar reasoning based on the number and strength of the acid sites also allows explaining the significantly higher activity of AuPd/CNTs-NS compared to AuPd/CNTs-N (Table 3), notwithstanding their similar particle size (Fig. 5B and D). In previous work, it was reported that too strong Brønsted acid sites are detrimental as they promote undesired acetalisation reactions of the intermediate pyruvic aldehyde.53 This was not the case with the catalytic system presented here, most likely because the Sn-MCM-41-XS used in combination with the Au–Pd catalysts provides enough Lewis acid sites to rapidly convert the pyruvic aldehyde formed after dehydration into the desired methyl lactate product (step C in Scheme 1).
In order to further prove the importance of using modified CNTs as support for the Au–Pd nanoparticles, the material consisting of Au–Pd nanoparticles supported on activated carbon using a similar CI method (average particle size = 9.9 nm, see Fig. 1B) was tested in combination with Sn-MCM-41-XS as catalyst for the conversion of glycerol to methyl lactate. A much lower activity was observed (9.3% glycerol conversion, see Table 3, entry 7), confirming the prominent role of the use of (functionalised) CNTs on the catalytic activity in this reaction. This lower activity can be ascribed to the larger size of the Au–Pd particles when AC is used as support (Fig. 1), which implies that a smaller fraction of the metal atoms are exposed on the surface and, therefore, are available as active sites. Moreover, the CNTs have different textural properties compared to AC. CNTs have fully open and thus more accessible external surface, whereas AC has a porous structure with large amount of micropores, which can cause mass transfer limitations of glycerol as well as of the reaction intermediates.
AuPd/CNTs was also tested without the addition of Sn-MCM-41-XS, leading to a much lower conversion of glycerol (Table 3, entry 8) and to poor selectivity towards methyl lactate (5.7%). The main by-products were MGo, DMO and MGe, all arising from over-oxidation of the initially formed trioses. This result indicates that Sn-MCM-41-XS plays an essential role by enhancing the rate of the rearrangement reactions of the trioses (and/or pyruvic aldehyde) and thus preventing over-oxidation of the trioses (Scheme 1), which can lead to the formation of inhibitors (e.g. glyceric acid, vide infra).15
The effect of the air pressure used during the catalytic test was investigated with the catalytic system consisting of AuPd/CNTs-S and Sn-MCM-41-XS (Fig. S3†). An almost identical catalytic performance (glycerol conversion around 71%) was observed with air pressure at 16 or 30 bar, whereas the conversion of glycerol dropped to 47% when the pressure was lowered to 10 bar. Based on the reaction stoichiometry, it was calculated that the minimum air pressure required for this reaction is around 8 bar. This indicates that when using 10 bar the reaction kinetics depends on air pressure, whereas it becomes 0th order when the pressure is 16 bar or higher. To get a deeper insight in the kinetics of this reaction, the conversion of glycerol and selectivity to the major intermediates/products was determined as a function of the batch time for the catalytic system consisting of AuPd/CNTs-S and Sn-MCM-41-XS (Fig. 6). The conversion of glycerol increased almost linearly in the first 4.5 h and reached 85% after 15.5 h. The selectivity to methyl lactate was nearly constant at around 90% between 0 and 15.5 h. The main by-product was MGe with a selectivity of around 6%, while the selectivity towards other products were all below 2%. The initial conversion of glycerol (0–4.5 h) was analysed by plotting the natural logarithm of the concentration of glycerol vs. reaction time. The linear fitting gave a R2 value of 0.994, which suggests a first order reaction with respect to glycerol concentration. This fact, in combination with the constant selectivity towards methyl lactate throughout the reaction, points to the initial partial oxidation of glycerol as the rate determining step under the employed reaction conditions. Compared to the initial stage of the reaction, the conversion of glycerol at the second half stage (4.5–15.5 h) only had a slow increase from 68% to 84%, whereas the selectivity to methyl lactate stayed identical (Fig. 6). For this later stage of the reaction, the slope of the natural logarithm of the concentration of glycerol vs. the reaction time is much lower than for the initial stage (Fig. S4†). This indicates that the reaction is no more first order with respect to glycerol concentration and suggests that partial inhibition of the catalyst by reaction intermediates or products might occur. To investigate this potential inhibition of the catalytic activity, a number of tests were performed by including possible reaction intermediates (methyl esters and their corresponding carboxylic acids) in the initial reaction mixture, using a molar ratio of 9 to 1 between glycerol and additional compound (Fig. S5†). The tests carried out in the presence of 10% of methyl esters (glycolate, oxalate or formate) gave similar results to the reaction without any additional compound. However, when performing the experiments in the presence of 10% of the corresponding carboxylic acids (glycolic acid, oxalic acid or formic acid), a clear reduction of the glycerol conversion was observed (Fig. S5†). The effect was even more marked when 10% glyceric acid was employed in the system, leading to a decrease in the conversion of glycerol from 54% to 12% with a dramatic drop in the selectivity towards methyl lactate from 90% to 28%. The inhibition effect by glyceric acid was similar even when only a small amount (2% relative to glycerol) was added to the reaction mixture. On the other hand, the activity only slightly decreased upon the addition of 2% lactic acid. The effect of adding a strong inorganic acid such as H2SO4 (0.05 mM) was also studied: the activity decreased from 54% to 22% but the selectivity towards methyl lactate was not affected. These results prove that the methyl esters of the by-products do not affect significantly the catalysts, whereas the corresponding carboxylic acids, and particularly glyceric acid, negatively affect the catalytic system. Since small amounts of H2O were generated from the oxidation of alcohols and the dehydration of pyruvic aldehyde (Scheme 1), the methyl esters in the reaction mixture may partially hydrolyse to form carboxylic acids. These carboxylic acids probably compete with glycerol in the adsorption on the catalytic surface and thus inhibit the catalytic activity.15 This phenomenon is reversible, as proven by the high reusability of the catalytic system consisting of AuPd/CNTs-NS and Sn-MCM-41-XS.
For the recycling experiments, the catalyst was separated from the reaction mixture, washed and dried and subsequently re-used for another run. The results show that the activity and selectivity are virtually constant in 5 consecutive runs (Fig. 7), demonstrating excellent catalyst reusability under the operating conditions. The elemental composition of the catalysts was analysed by ICP-OES after 5 runs and did not reveal any changes in the Au/Pd molar ratio in AuPd/CNTs-NS or in the Si/Sn molar ratio in Sn-MCM-41-XS (Table S2†). Moreover, the catalyst reused in 5 consecutive runs was analysed by TEM (Fig. S6†) and showed a very similar average particle size (3.8 nm) compared to the fresh catalyst (3.5 nm, Fig. 5D). The TEM image also revealed that AuPd/CNTs-NS and Sn-MCM-41-XS were intimately mixed, the distance between them being at the nanoscale, which is beneficial for the mass transfer of reactants and intermediates during the reaction. These results indicate that there was negligible change in the catalyst after 5 runs, which correlates well with the observed reusability with no activity loss.
The multi-walled carbon nanotubes were functionalised by oxidation using H2O2, HNO3, H2SO4 or HNO3–H2SO4. A representative experimental procedure for the CNTs treatment by H2O2 (CNTs-O) is as follows: CNTs (2.5 g) were suspended in an aqueous H2O2 solution (30 wt%, 25 mL) and the mixture was sonicated for 30 min. The mixture was then refluxed at 65 °C for 6 days while adding a fresh aqueous H2O2 solution (30 wt%, 10 mL) every 12 h (120 mL in total). Next, the suspension was filtered and the solid residue was washed with MilliQ water until the filtrate was neutral. The obtained solid was dried at 100 °C overnight. A representative procedure for CNTs treatment by HNO3 (CNTs-N) is as follows: CNTs (2.5 g) were suspended in an aqueous solution of HNO3 (30 wt%, 50 mL). The mixture was sonicated for 30 min, after which it was refluxed for 2 h by setting the temperature of the oil bath at 140 °C. The suspension was filtered and the solid residue was washed with MilliQ water until the filtrate was neutral. The obtained solid was dried overnight at 100 °C. A representative procedure for CNTs treatment by H2SO4 (CNTs-S) is as follows: CNTs (2.5 g) were suspended in an aqueous solution of H2SO4 (98%, 25 mL) and the mixture was sonicated for 30 min. The mixture was then refluxed by setting the temperature of the oil bath at 150 °C for 15 h. The reaction mixture was diluted with MilliQ water, after which it was filtered and washed with MilliQ water. The resulting solid was dried overnight at 100 °C. A representative procedure for CNTs treatment by HNO3–H2SO4 (CNTs-NS) is as follows: CNTs (2.5 g) were suspended in a mixture of aqueous HNO3 (30 wt%, 25 mL) and H2SO4 (98%, 25 mL) and the slurry was sonicated for 30 min. The mixture was then maintained at 60 °C for 15 h. Next, the reaction mixture was diluted with MilliQ water, after which it was filtered and washed with MilliQ water. The resulting solid was dried overnight at 100 °C.
Mono- and bimetallic Au–Pd catalysts supported on CNTs were prepared using a colloidal immobilisation (CI) method aiming at a theoretical metal loading of 1 wt%.30 The preparation of Au–Pd NPs (1 wt%) supported on the chosen type of CNTs with a molar ratio of Au-to-Pd of 1 was as follows: an aqueous HAuCl4 solution (3.5 g Au per L, 1.85 mL), an aqueous PdCl2·2HCl solution (3.5 g Pd per L, 1.00 mL) and 2 wt% of an aqueous PVA solution (1.2 mL) were added to MilliQ H2O (100 mL) and the mixture was stirred for 30 min at room temperature. A freshly prepared aqueous solution of NaBH4 (0.1 M, 2.54 mL) was added dropwise to the mixture, which was then stirred for 30 min. The pH was set to 2 by the addition of an aqueous H2SO4 solution (1 M). Subsequently, CNTs (1 g) were added to the solution. The CNTs were sonicated (30 min) in MilliQ water (50 mL) prior to use, to achieve a good dispersion. The suspension was stirred for 2 h and subsequently filtered. The residue was washed with H2O (2 L) to neutralise the mixture and to remove PVA. Finally, the solid was dried overnight at 80 °C.
Sn-MCM-41-XS was synthesised according to a previously reported method.20 In short, an aqueous solution of NaOH (2 M, 3.6 mL) was added to a solution of CTAB (1.0 g) in H2O (480 mL), after which the mixture was stirred vigorously at room temperature for 30 min. Next, TEOS (2.29 g) was added dropwise to this solution. Then, a solution of SnCl4·5H2O in ethanol (0.3 M, 1 mL) was added dropwise, after which more TEOS (2.29 g) was added dropwise. After stirring the mixture at room temperature for 2 h, the white gel was filtered and washed three times with MilliQ H2O (10 mL) and then with ethanol (10 mL). The obtained white solid was dried at 70 °C overnight and the resulting powder was calcined at 550 °C in air for 5 h, with a heating rate of 3 °C min−1. The following molar ratio was used: 1 TEOS:0.0135 SnCl4·5H2O:0.33 NaOH:0.125 CTAB:0.9 EtOH:1247 H2O. See Fig. S7† for selected characterisation data for Sn-MCM-41-XS.
The glycerol conversion (Conv./%) is defined by eqn (1):
(1) |
The product selectivity for a compound P is defined by eqn (2):
(2) |
The carbon balance (C/%) was calculated as the sum of the concentration of unreacted glycerol and of the yields of all products detected by GC.
For the catalysts recycling tests, after a small amount of the reaction mixture was collected for analysis at the end of the catalytic test, the remaining mixture was filtered and the catalysts were recovered. The catalysts were washed first with MilliQ H2O (20 mL), then with ethanol (20 mL), and this procedure was repeated 3 times, after which the solid was dried overnight at 100 °C. This solid was used for another batch experiment.
Nitrogen physisorption isotherms were measured at −196 °C using a Micromeritics ASAP 2420 apparatus. The Brunauer–Emmett–Teller (BET) method was employed to calculate the specific surface area. The Barrett–Joyner–Halenda (BJH) method was used to calculate the pore volume.
Inductively-coupled plasma optical emission spectrometry (ICP-OES) was performed using a PerkinElmer Optima 7000 DV instrument in order to obtain the actual Au and Pd loadings on the supports, as well as the actual Si/Sn ratio in Sn-MCM-41-XS.
Energy-dispersive X-ray spectroscopy (EDX) measurements were performed on a FEI Tecnai T20 electron microscope operating at 200 keV with an Oxford Xmax 80T detector. The samples were prepared by ultra-sonication in ethanol followed by drop-casting of the material on a copper grid.
X-ray Photoelectron Spectroscopy (XPS) was measured by mounting the catalysts on a conductive tape attached to the XPS sample holder. No further treatment was carried out prior to the XPS measurement. The measurements were performed using a Surface Science SSX-100 ESCA instrument equipped with a monochromatic Al Kα X-ray source (hν = 1486.6 eV) and operating at a pressure below 2 × 10−9 mbar. The analysed spot size was 600 μm; an electron flood gun was employed to compensate for charging effects. Spectral analysis included Shirley background subtraction54 and peak deconvolution using the Winspec software package developed by LISE laboratory, University of Namur, Belgium. Binding energies were referenced to the C 1s peak set at 284.5 ± 0.2 eV.
The amount of acid sites per gram of CNTs was measured by Boehm titration.50 For this test, a CNTs sample (0.2 g) was added to an aqueous basic solution of NaHCO3 (0.05 M, 25 mL) to determine the stronger acid sites, such as carboxylic and sulphonic acid groups; or to an aqueous solution of NaOH (0.1 M, 25 mL) to determine the total amount of acid sites. The suspensions were stirred for 24 h at room temperature and filtered before titration. Aliquots (10 mL) of the filtered solutions were titrated with 0.1 M HCl.
The dispersibility of the functionalised CNTs was evaluated by suspending the CNTs (20 mg) in water (20 mL) using ultra-sonication for 30 min. The mixture was stored without agitation for 1 week. Then, one drop of the suspension was taken and dropped on a filter paper to visually determine the state of aggregation of the functionalised CNTs.
Footnote |
† Electronic supplementary information (ESI) available: Comparison with previously reported heterogeneous catalysts, correlation between oxygen content and number of total acid sites, dispersion of functionalised carbon nanotubes, conversion of glycerol at different reaction pressures, plot of the concentration of glycerol as a function of the reaction time, conversion and selectivity as a function of the addition of different compounds, TEM pictures of the used catalysts, elemental analysis of the used catalysts, TEM picture of Sn-MCM-41-XS. See DOI: 10.1039/c9gc01521c |
This journal is © The Royal Society of Chemistry 2019 |