Meng
Jin‡
a,
An-Zhen
Li‡
a,
Ye
Wang
a,
Jing
Li
a,
Hua
Zhou
b,
Bi-Jie
Li
*a and
Haohong
Duan
*ac
aDepartment of Chemistry, Tsinghua University, Beijing 100084, China. E-mail: bijieli@mail.tsinghua.edu.cn; hhduan@mail.tsinghua.edu.cn
bState Key Laboratory of Chemical Resource Engineering, College of Chemistry, Beijing University of Chemical Technology, Beijing 100029, China
cHaihe Laboratory of Sustainable Chemical Transformations, Tianjin 300192, China
First published on 10th July 2023
N,N-Dimethylformamide (DMF) is a universal solvent with wide applications across various industries. Current industrial synthesis requires high temperature and high pressure, starting from fossil-based carbon monoxide and dimethylamine (DMA). Herein, we report a green and electrochemical strategy to produce DMF under ambient conditions through direct oxidation of trimethylamine (TMA), which is a surplus chemical in DMA manufacturing. DMF production with 80% yield and >50% faradaic efficiency was achieved in an H-cell reactor over a graphite anode, coupled with hydrogen production at the cathode. Mechanistic investigations show that the reaction occurs through two-phase oxidation and that an aminal serves as the key intermediate. To achieve continuous DMF production, we set up a membrane-electrode assembly (MEA) flow reactor (2 cm × 2 cm), achieving a DMF productivity of 25 μmol h−1 and a faradaic efficiency of 40%. To further increase the productivity, we fabricated another membrane-free flow reactor (8 cm × 9 cm), delivering a high formation rate (550 μmol h−1) with high selectivity (>90%) at a constant current of 3 A in a 100-hour test. This study offers a unique opportunity to utilize electricity to drive surplus chemical utilization under ambient conditions, contributing to the sustainability of the chemical industry in the future.
Scheme 1 Design concept. (a) Manufacture of methylamine products in industry. (b) Industrial DMF synthesis. (c) Electrochemical synthesis of DMF from TMA. |
Industrially, DMA is synthesized through methanol amination,8 but monomethylamine (MMA) and trimethylamine (TMA) are simultaneously generated with much lower market values compared to DMA (Scheme 1a). It is feasible to recycle MMA for DMA production; nevertheless, it is more difficult and costly to recycle TMA. Moreover, TMA is thermodynamically more favourable than the other two amines, with an equilibrium ratio of MMA:DMA:TMA close to 17:21:62 (when the ammonia:methanol molar ratio is 1:1).9,10 Consequently, the large TMA distribution in the products greatly limits the overall efficiency for DMA production. Although advanced silica–alumina catalysts were reported to suppress TMA formation via methanol animation to some extent,11–13 the development of a cost-effective and less energy-intensive method to directly channel TMA into DMF production is desirable to enhance the synthetic efficiency of DMA.
To fill this gap, we envisage that direct TMA oxidation to DMF would be a green and economically promising route. The direct oxidation of amines to amides is a particularly useful process in organic synthesis due to the widespread occurrence of amides across diverse organic molecules.14 This oxidation is usually achieved through thermocatalytic15–17 or photocatalytic18–20 approaches, where metal catalysts, hazardous oxidants or special additives are usually necessary. More importantly, this oxidation usually occurs preferentially at the α secondary carbon instead of the primary carbon with few exceptions,21,22 because of the stability of the corresponding secondary carbon radical. As a result, due to the low boiling point, stronger methyl C–H bonds and formation of side-products such as trimethylamine oxide,23 the conventional approaches have rarely been successfully applied to TMA oxidation.23–25
(1) |
Electrosynthesis of value-added chemicals and fuels has emerged as a green and sustainable method,26–33 for its ambient conditions (e.g., room temperature and ambient pressure) and the use of renewable electricity (e.g., solar, wind, hydro).34 Based on our research interest in the electrosynthesis of valuable chemicals from biomass- and plastic-derived compounds,35–37 we recently questioned whether an electrochemical method can be developed to accomplish the direct oxidation of TMA to DMF. If successful, this process will generate value-added chemicals at the anode, with an additional benefit of simultaneous hydrogen (H2) production at the cathode, a green energy carrier with a large market demand.38,39 Although the Shono-type reaction indicates that amines and carbamates can be oxidized at the anode,40 additives (Lewis acids,41 aminoxyl mediators42–44 and halide ions45) are necessary, in which the Lewis acid mediates the generation of a reactive iminium ion intermediate, while aminoxyl mediators and halide ions serve as the redox mediators. The use of these additives may increase the product separation cost and feedstock cost, thus restricting the practical applications. In addition, the Shono-type reactions are often conducted in organic solution, while aqueous solution is environmentally more desirable. According to eqn (1), direct electrochemical oxidation of TMA to DMF is a multi-proton and multi-electron process (4e− and 3H+ are transferred); thus the challenge lies in the development of an efficient electrochemical system without any mediator and using only water as the oxidant to achieve high selectivity of DMF at a moderate potential.
Herein, we report an electrochemical oxidation strategy to synthesize DMF directly from TMA, which was conducted at ambient temperature and pressure in an aqueous medium without any additives (Scheme 1c). DMF production with 80% yield and >50% faradaic efficiency (FE) was achieved over cost-effective graphite as the anode, coupling with hydrogen production using platinum (Pt) or nickel (Ni) as the cathode. Mechanistic investigations show that a two-phase oxidation is involved, where an aminal serves as the key intermediate for producing DMF. To achieve continuous DMF production, we set up a membrane-electrode assembly (MEA) flow reactor (2 cm × 2 cm), with a DMF productivity of 25 μmol h−1 and a faradaic efficiency of 40%. To further increase the productivity, we fabricated a membrane-free reactor (8 cm × 9 cm) in a single module. In a 100-hour test, a high formation rate (550 μmol h−1) with high selectivity (>90%) at an absolute current of 3 A was maintained. Moreover, a high DMF yield (75%) was obtained in the flow reactor by circulating the electrolyte, and the performance is recyclable without activity loss. In addition, calculations of several important green chemistry metrics—including atom economy (AE), environmental factor (E-factor), and carbon efficiency (CE)—suggest that this method represents a potentially green route to produce DMF.
Entry | Catalyst | Electrolyte | Yield (%) | FE (%) |
---|---|---|---|---|
a Reaction conditions: graphite flake anode (1 cm × 1 cm), Pt cathode (1 cm × 1 cm), TMA (0.1 mmol), water (5 mL), at 1.1 V vs. Hg/HgO for 2 h at room temperature in an H-type cell. | ||||
1 | Graphite flake | 0.7 M KOH | 16 | 2 |
2 | Graphite flake | 0.7 M K 2 CO 3 | 80 | 56 |
3 | Graphite flake | 0.7 M KH2PO4 | 22 | 21 |
4 | Graphite flake | 0.7 M PBS | 19 | 7 |
5 | Graphite flake | 0.7 M KCl | 5 | 6 |
6 | Graphite flake | 0.1 M K2CO3 | 50 | 37 |
7 | Graphite flake | 1.5 M K2CO3 | 66 | 41 |
The electrolyte was further optimized using graphite flake as the anode (entries 1–5, Table 1), and K2CO3 delivers the highest DMF yield (entry 2, Table 1). Although complete TMA conversion was observed when KOH was used as the electrolyte, DMF yield was only 16% for 2 h (entry 1, Table 1). With the reaction time extended to 5 h, the DMF yield decreased to 1%, indicating that the use of KOH as the electrolyte probably caused TMA overoxidation or decomposition (Fig. S7†). Low TMA conversions and DMF yields were observed in KH2PO4, PBS and KCl (entries 3–5, Table 1). Based on K2CO3 as the optimal electrolyte, we found that either decreasing (entry 6, Table 1) or increasing (entry 7, Table 1) the K2CO3 concentration reduced the DMF yield. We recognize that electrolyte pH also greatly affects DMF selectivity. By adding 0.7 M KOH into 0.7 M K2CO3 (to increase pH), or adding 0.7 M KHCO3 into 0.7 M K2CO3 (to decrease pH), lower selectivity and FE of DMF were obtained compared with that in 0.7 M K2CO3 with pH 12.2 (Fig. S8†). Based on the above optimizations, using graphite flake as the anode, Pt as the cathode, and 0.7 M K2CO3 with 20 mM TMA as the electrolyte, the efficient electrochemical oxidation of TMA to DMF was realized (DMF yield of 80% and FE of 56%, shown in entry 2, Table 1) in an aqueous medium without any additives under ambient temperature and pressure. These are set as the standard conditions for the following evaluations.
We then investigated the effect of applied potential on product selectivity. According to the potential range shown in the LSV curve, we performed the reaction at a constant potential from 0.9 to 1.3 V vs. Hg/HgO (Fig. 1c and Table S3†). In the potential range of 0.9–1.1 V vs. Hg/HgO, the DMF yield and FE gradually increased with the increase of potential (Fig. S9a†), while formaldehyde's FE decreased. It is speculated that a slow reaction rate at lower potential may be caused by the accumulation of formaldehyde as a reaction intermediate (discussed later). The DMF yield and FE are the highest when the potential is increased to 1.1 V vs. Hg/HgO (entry 2, Table 1). However, when the potential was further increased to 1.3 V vs. Hg/HgO, both DMF yield and FE significantly decreased. The yield continued to decline with the extension of reaction time, indicating overoxidation of DMF (Fig. S9b†) and the intermediates, as well as the competition of the OER at the high potential (Table S4†). At the same time, it also caused a significant decrease in the faradaic efficiency.
To further understand the reaction mechanism of the electrochemical oxidation of TMA to DMF, differential electrochemical mass spectrometry (DEMS) experiments were carried out to detect the reaction intermediates. The measurement was carried out in the undivided cell, containing 0.7 M K2CO3 with 20 mM TMA, using carbon paper, Pt wire, and Hg/HgO as the working, counter, and reference electrodes, respectively. The DEMS was performed under the standard conditions, as shown in Fig. 2b. The signal with a mass-to-charge ratio (m/z) of 59 kept decreasing, which is assigned to TMA consumption during the reaction. Another signal with a m/z of 45 first increased and then decreased over time, which is assigned to DMA, indicating its generation and then consumption during the measurement. These results are consistent with the above time course study (Fig. 2a). It is reported that during the oxidation of amines to amides, aminal intermediates are formed.50,51 However, the formation of DMF and other reaction intermediates including aminal intermediates was not observed, probably due to their low vaporization ability or instability under the tested conditions. Furthermore, in situ infrared reflection absorption spectroscopy (IRRAS) (Fig. 2c) was conducted in 0.7 M K2CO3 with 20 mM TMA at 1.1 V vs. Hg/HgO for 1200 s. With the prolonging of the reaction time, the peaks at 1670 cm−1 and 1755 cm−1 can be assigned to the vibrational stretching of carbonyl (CO), which could be attributed to the formation of DMF and formaldehyde.52
According to the above analysis that DMA and formaldehyde are formed during the electrochemical oxidation of TMA to DMF, we speculate that TMA might be initially oxidized to an aminal intermediate ((CH3)2NCH2OH), which is then reversibly transformed to DMA and formaldehyde, or further oxidized to DMF. Because the nucleophilic attack of a hydroxide (HO−) to N,N-dimethylmethyleneiminium iodide (namely, Eschenmoser's salt) would generate a (CH3)2NCH2OH intermediate, an electrochemical test was performed using Eschenmoser's salt as the substrate in order to demonstrate that an aminal could be the reaction intermediate. The results show that DMF was obtained in 78% yield (Scheme 2b); therefore (CH3)2NCH2OH is presumably involved as the reaction intermediate. This also explains the higher FE of formaldehyde at lower pH, because the lower pH would promote hydrolysis of the aminal (Fig. S8†).
In order to gain more insights into the reaction mechanism, radical trapping experiments were performed. A decreased yield of DMF after adding 5,5-dimethyl-1-pyrroline N-oxide (DMPO, 15% decrease in yield with 10 mM DMPO, and 25% decrease in yield with 20 mM DMPO, Fig. S11†) was observed, indicating that a radical pathway through a single-electron transfer (SET) process was involved. To further confirm our conjecture, the possible formation of free radicals during the reaction was detected by electron paramagnetic resonance (EPR) study. The measurement was conducted in 0.7 M K2CO3 with 20 mM mmol TMA using 100 mM DMPO as the trapping reagent. Prior to the measurement of EPR, the reaction solution was subjected to constant potential electrolysis (1.1 V vs. Hg/HgO) for 6 minutes to initiate the reaction. The typical signals of ˙C, ˙OOH and 1O2 were detected (Fig. 2d). We speculate that ˙C is attributable to a dimethylaminomethyl radical formed by TMA oxidation,53 and then dimethylaminomethyl radical can be oxidized to an iminium ion and finally to DMF. In addition, ˙OOH and 1O2 radicals are possibly formed by the electrooxidation of water, but they exhibit an insignificant effect on DMF formation. To confirm the role of ˙C radical in DMF formation, we conducted the EPR experiment under reaction conditions with KCl as the electrolyte, in which a much lower DMF yield was obtained (entry 5, Table 1). The radical signal of ˙C with much weaker intensity was observed (Fig. S12†), indicating that the ˙C radical is an intermediate during the electrochemical oxidation of TMA to DMF.
Based on the above discussions and previous studies,54,55 we propose that the electrochemical oxidation of TMA to DMF proceeds through the following pathway (Scheme 3). TMA (1) is initially oxidized to an amino radical cation (1a) via single electron transfer (SET). 1a is then deprotonated to give an α-amino carbon radical (1b). 1b is then oxidized to an iminium intermediate (1c) via another SET process. Upon nucleophilic attack by OH− in the electrolyte, aminal (2a) is formed, with a reversible transformation to DMA (2b) and formaldehyde (2c). Finally, 2a is oxidized to DMF (2) through 2e− and 2 proton transfer processes. Overall, TMA is electrochemically oxidized to DMF via the above 4e− and 3H+ transfer process without using any mediators.
Similar to the results shown in the aforementioned H-cell reactor, the applied voltage is a key factor influencing DMF productivity and FE. We thus varied the applied voltage from 2.0 V to 2.5 V (Fig. 3d) in the MEA flow reactor. The results show that DMF productivity and FE are relatively low under a lower voltage, and high selectivity of formaldehyde is obtained, which is an indication of the slow oxidation of the aminal intermediate at the lower voltage (Fig. S14†). The productivity of DMF increased at increased voltages, but FE decreased due to the competition of the OER. After preliminary optimization of the applied voltage, we achieved continuous DMF electrosynthesis with a productivity of 26 μmol h−1 and FE of 40% at 2.2 V. Then a 20-hour i–t test was conducted to evaluate the stability of this MEA flow reactor-based system. Under a cell voltage of 2.1 V, the solution of 0.7 M K2CO3 with 20 mM TMA was circulated into the MEA flow reactor with a flow rate of 5.4 mL min−1. A relatively stable current density (ca. 2 mA cm−2) and FE of DMF (ca. 38%) were achieved in the 20-hour test (Fig. S15†), indicating high stability.
To further increase DMF productivity to meet more practical-relevant scenarios, a two-electrode, membrane-free flow reactor was conceived (Fig. 4a) and set up (Fig. 4b and Fig. S16†). By not using a membrane (AEM), although ohmic resistance would increase, the reactor would be more cost-effective, thus being conducive to scaling up the reactor in more practical scenarios. Due to the high cost of Pt, and also the comparable activity of Ni foam as the cathode (tested in a membrane-free flow reactor with a smaller working electrode area of 4 cm2, Fig. S17†), Ni foam was used as the cathode in the membrane-free flow reactor (8 cm × 9 cm). Compared with MEA, the membrane-free flow reactor has one feed inlet and one discharge outlet, so the resulting gas–liquid is mixed at the discharge outlet. Optimization of TMA concentration and flow rate was then performed (Fig. S18†). The DMF productivity was higher in 0.7 M K2CO3 with 200 mM TMA at a flow rate of 5.4 mL min−1. The LSV curve (Fig. S19a†) shows that TMA oxidation takes place from a cell voltage of approximately 1.9 V, and the current density reached 100 mA cm−2 at 2.5 V. The voltage is lower than that in 0.7 M K2CO3 without TMA, suggesting that TMA oxidation is preferable to the OER. This is consistent with the results in the aforementioned investigations in the H-cell and MEA flow reactors. We then demonstrated that DMF can be produced in a high yield using this membrane-free flow reactor. The electrolyte passes through the flow reactor with circulation, and the products (and the unreacted TMA) were immersed in an ice-bath to prevent TMA from evaporation considering its low boiling point (ca. 3 °C). Eventually, DMF was obtained in a high yield (75%) in a 24-hour test (Fig. 4c). Moreover, the system can be reused three times without activity loss, demonstrating the reusability of the flow system.
We then evaluated the robustness of this flow system in a long-term operation, which is a prerequisite for practical applications. The device was continuously operated for 100 hours without a noticeable change in DMF selectivity (roughly 98%) or cell voltage (roughly 2.6 V). During this stability test, the formation rate of DMF was maintained relatively constant at around 550 μmol h−1 (Fig. 4d). Unfortunately, the FE of DMF was low (approximately 2%, Fig. S19b†), much lower than that obtained in the H-cell or MEA flow reactors. This is not unreasonable considering the large working area of the membrane-free reactor, on which TMA diffusion would be more difficult, which in turn results in intense OER. These results indicate that the reactor design with a large working area may become a decisive factor in determining the reaction efficiency, which is worth investigating for scaling-up electrosynthesis. Further optimizations of the MEA flow reactor and membrane-free reactor are ongoing in our laboratory.
Eventually, we assessed green chemistry metrics and profitability of electrochemical synthesis of DMF from TMA shown in this work. Regarding green chemistry characteristics, we performed calculations on several important green chemistry metrics, including the AE, E-factor, and CE. The calculation details of these green chemistry metrics are shown in the ESI (Tables S5 and S6).† The calculation results of the electrochemical synthesis of DMF display high AE (94.8%), low E-factor (4.62), and high CE (88%), indicating that the synthetic method is potentially green and sustainable. Regarding profitability, we conducted a preliminary techno-economic analysis (TEA) (full details of the TEA are available in the ESI, Fig. S20†). The results suggest that the profitability of the process depends on the cost of renewable electricity, operating current density and FE of DMF. With the development of renewable electricity in the future, its cost continues to plummet to below 10 cents kW h−1.57 In this context, the electrochemical oxidation of TMA to DMF is economically possible when the system achieves a certain FE (>30%) and current density (>100 mA cm−2). While there is still a substantial gap between the low FE we obtained and the desirable profitability requirement, continuous DMF production with a high current and long-term stability suggests the potential of the electrochemical strategy.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3gc01406a |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2023 |