Jun Hyuk
Kim
,
Kyuseon
Jang
,
Dae-Kwang
Lim
,
Sejong
Ahn
,
DongHwan
Oh
,
Hyunseung
Kim
,
Jongsu
Seo
,
Pyuck-Pa
Choi
and
WooChul
Jung
*
Department of Materials Science and Engineering, KAIST, Daejeon, Republic of Korea. E-mail: wcjung@kaist.ac.kr
First published on 26th November 2021
The oxygen reduction reaction, which proceeds at the cathode of a fuel cell, is primarily important as its rate determines the overall performance of a device. However, designing a single-phase material that meets multiple standards (e.g., high activity, stability, and thermomechanical characteristics) at once to become an ideal cathode still remains a great challenge. In this regard, the use of multi-phase catalysts, especially those with complex nanoscale domains, may serve as a rational strategy. Here, we present Ba0.5Sr0.5Co0.6Fe0.2Zr0.1Y0.1O3−δ (BSCFZY) as a superior biphasic nano-composite cathode, which self-assembles into two discrete cubic perovskites: Co-rich (Ba0.5Sr0.5Co0.7Fe0.2Zr0.07Y0.03O3−δ) and Zr-rich (Ba0.6Sr0.4Co0.3Fe0.2Zr0.4Y0.1O3−δ) phases. The former promotes the electrocatalytic activity while the latter supports the microstructural robustness; thus, the synergic ensemble of Co- and Zr-rich perovskite domains yields an area specific resistance of only ∼0.013 Ω cm2 at 650 °C, which is far superior to that anticipated from the component phases in isolation. The cooperative interaction found in multi-phase catalysts prepared via a simple one-pot synthesis is not only attractive for SOFCs but also for other kinds of energy conversion and storage devices, such as protonic ceramic electrochemical cells, electrolysers, and membrane chemical reformers.
The strategy has proven viable when used with a solid oxide fuel cell (SOFC) as well.8 As an eco-friendly power source, a SOFC represents one of the most competitive options to convert chemical fuels into electricity in a clean and sustainable manner.9–14 Generally, power generation by the device hinges critically on the oxygen reduction reaction (ORR) rate; hence, a grand overarching goal for researchers has been the development of a high-performance cathode.15–17 For this purpose, composite electrodes have been routinely employed in the field of SOFCs, which are, in fact, a form of multi-phase catalyst. For instance, La0.8Sr0.2MnO3 (LSM)-yttria-stabilized-zirconia (YSZ) is a commercially available composite cathode where each phase plays different roles; LSM acts as an electronic conducting phase and YSZ acts as an ionic conducting phase. Often, these multi-phase electrodes are prepared by physical mixing methods such as ball-milling, and even if possible, these offer only limited processability at the nanoscale. Formulating nanoscale composite electrodes has important merits, as the better homogeneity of mixing can expand the effective cathodic reaction regions, leading to a superior activity.18–22 Moreover, nano-structured materials endorse high porosities advantageous to the efficient gas transport. Hence, a method to obtain nano-composites is highly desirable, however often these methods are time-consuming or accompany highly energy-intensive processes, which are not practically applicable in large-scale.
In this light, nano-composites prepared via a self-assembly process are emerging as an attractive option, as multi-phase catalysts can be obtained by a single heat treatment at relatively low calcination temperatures.8,23–25 In addition to this processing advantage, self-assembled materials have been found to be potential cathode candidates, evidenced by their high activity, decent chemical and physical compatibility with electrolytes, and their robust structural stability, empowered by the combination of advantageous characteristics of each distinct phase. While the design rules for the self-assembly process are not fully understood yet, as a rule of thumb, excessive B-site doping of Mo, W, Ce and Zr ions into Co and Fe-based perovskites holds high chances to yield phase separation as these elements exhibit low solid-solution compatibility.24,26–29 For example, Shin et al. carefully designed Ba0.5Sr0.5(Co0.7Fe0.3)0.6875W0.3125O3−δ (BSCFW), a composite which consists of W-rich double perovskites and W-poor single perovskites.24 In this composite, W-rich double perovskites provided an inert and rigid support to active phases (i.e., W-poor single perovskites), which significantly augmented the thermal stability of the material. Similarly, Song et al., reported Sr0.9Ce0.1Fe0.8Ni0.2O3−δ (SCFN) which consists of 4 different phases: perovskite, Ruddlesden–Popper (RP), NiO, and CeO2. Each domain has its characteristic role in enhancing the electrode performance;23 the perovskite phase functions as a mixed-conducting backbone, while RP, NiO and CeO2 promoted the oxygen bulk diffusion, oxygen surface exchange, and oxygen migration respectively. Meanwhile, Chen et al. reported that multi-phase catalyst coatings can dramatically improve the performance of the conventional La0.6Sr0.4Co0.2Fe0.8O3−δ cathode, due to the accelerated oxygen adsorption and dissociation on BaCoO3−δ nanoparticles.8 As shown above, self-assembled multi-phase catalysts represent salient progress toward the rational design of advanced cathodes for SOFCs.23,26,30,31
Inspired by these recent advances, here we present Ba0.5Sr0.5Co0.6Fe0.2Zr0.1Y0.1O3−δ (BSCFZY) as a self-assembled hybrid catalyst capable of rapid oxygen reaction kinetics. The composition of BSCFZY includes two paradigm-shifting cathode materials: Ba0.5Sr0.5Co0.8Fe0.2O3−δ (BSCF) and BaCo0.4Fe0.4Zr0.1Y0.1 (BCFZY).32,33 BSCF is highly conducting and active toward oxygen-electrochemistry, but it comes with the caveat of questionable durability.24,34 On the other hand, BCFZY exhibits exceptional stability and a relatively low thermal expansion coefficient (2.16 × 10−5 K−1), but the low electronic conductivity (∼1 S cm−1) of the material can be a concern when current collecting is not well managed.35,36 Hence, we make an effort to merge the key merits of these two cathodes via a self-assembly process. By leveraging the sinter-resistance of the Zr-containing phase, perovskites of different compositions are efficiently yielded as nano-composites within a single calcination process. The resulting multi-phase cathode demonstrates outstanding ORR performance, excellent stability, and a moderate thermal expansion coefficient mismatch to the electrolyte, suggesting that the developed material system is a highly reliable and practical candidate for use in SOFC cathodes.
To validate these outcomes, the BSCFZY powder was investigated using scanning transmission electron microscopy (STEM) and by means of an energy-dispersive X-ray (EDX) analysis (Fig. 1b, c, S3 and S4†). Notably, it was found that BSCFZY consists of nanograins with an inhomogeneous distribution of the Zr element according to EDX scans (Fig. 1f and g) of points 1 and 2 (Fig. 1c), signifying variations of the compositions between the two phases. Indeed, high-resolution transmission electron microscopy (HRTEM) images of each phase (Fig. 1d and e) show different diffraction planes, supporting multi-phase formation through the self-assembly process.
Although both STEM-EDX and XRD indicate the presence of two distinct phases in the powder, it is difficult to determine the accurate composition of these phases due to the overlap of EDX signals between Sr, Y, and Zr. We thus conducted atom probe tomography (APT) to investigate the composition and three-dimensional entanglement of the two phases at the atomic scale. APT is the only material analysis technique offering extensive scope for both 3D imaging and chemical measurements on the atomic scale with sub-nanometer resolutions. Details about the APT measurements are shown in Fig. S5.†Fig. 2a shows a three-dimensional atom map acquired from the BSCFZY powder. The measured bulk composition of the entire probed volume is Ba0.5Sr0.5Co0.6Fe0.2Zr0.1Y0.1Ox, in good agreement with the target composition of the as-synthesized powder. Although atoms appear to be homogeneously distributed at first glance, the cross-sectional view reveals a Co-rich phase and Zr-rich phase (Fig. 2b). The proximity histogram obtained for the upper part with respect to the iso-concentration surface of Zr of 15 at% (see Fig. 2c), i.e., half of the maximum concentration of Zr in the Zr-rich phase, shows the change in elemental concentrations as a function of the distance from the boundary between Co- and Zr-rich regions (Fig. 2d). The opposed partitioning behavior of Co and Zr is consistent with the results obtained from EDX point scan analyses (Fig. 1f and g). The average compositions of the Co-rich and Zr-rich phases are analyzed as Ba0.5Sr0.5Co0.7Fe0.2Zr0.07Y0.03Ox and Ba0.6Sr0.4Co0.3Fe0.2Zr0.4Y0.1Ox, respectively, confirming the existence of multi-phase formation in BSCFZY powder (ratio of Zr- and Co-rich phases are ∼11.9% and ∼88.1% respectively, as obtained from XRD analysis).
The phase structure of the self-assembled perovskites is also characterized with in situ high-temperature XRD (Fig. 3a). Under the testing conditions (i.e., from room temperature to 700 °C), BSCFZY maintains its dual-phase nature, along with a slight peak shift to a lower angle. Hence the refined unit cell parameters of the Zr-BSCFZY and Co-BSCFZY phases are calculated and plotted as a function of the temperature (Fig. 3b). Due to the larger ionic radii of Zr4+ (86 pm) compared to those of other transition metals (Co3+: 75 pm and Fe3+: 78.5 pm), Zr-BSCFZY showed a larger lattice compared to that of Co-BSCFZY. As the temperature increases, the lattice expansion of both phases is observed, but with different slopes. The thermal expansion coefficients (TECs) of both phases are therefore analyzed by calculated the thermally expanded lattice parameters (Δa) divided by the lattice parameters at room temperature (a0). The resulting TEC values are obtained and found to be 1.90 × 10−5 K−1 for Co-BSCFZY and 1.36 × 10−5 K−1 for Zr-BSCFZY. The low TEC value of Zr-BSCFZY may be a representation of the fixed valence state of the Zr ions compared to the thermal reduction proceeding on Co/Fe ions, as shown by the thermogravimetric analysis (TGA, Fig. S6†).33,39 Regarding the ratio between the Zr- and Co-rich phases (∼11.9% and ∼88.1% respectively), the expected TEC value for BSCFZY is 1.83 × 10−5 K−1. Although the TEC of BSCFZY could not fully match the TEC of SDC (1.23 × 10−5 K−1) and GDC (1.20 × 10−5 K−1),40 compared to the conventional mixed-ionic-and-electronic-conducting cathodes which show a TEC range of 2.0–3.0 × 10−5 K−1,33,41–44 the TEC found for BSCFZY (1.83 × 10−5 K−1) is quite encouraging to use in our efforts to achieve good thermomechanical compatibility with SOFC electrolytes.
An additional characterization of X-ray photoelectron spectroscopy (XPS) is conducted to investigate the cation distribution/composition on the BSCFZY surface. Fig. S7† shows the photoelectron spectra of constituent cations in BSCFZY. Due to the direct overlap of Co 2p and Ba 3d, we used the Co 3p spectrum instead to fit the Co2+/Co3+ ratios. Accordingly, the amounts of Co3+ and Co2+ are determined to be approximately 68 and 32%, respectively. Similarly, the Fe 3p spectrum is deconvoluted with Fe3+ and Fe2+ peaks and the corresponding amounts are thus estimated to be close to 57 and 43%. Finally, we examined the XPS spectra of Sr 3d for BSCFZY, with the doublets (3d3/2 and 3d5/2) of both Srnon-lattice and Srlattice assigned to deconvolute the spectra. Particularly, it is reported that the peak positions of Srnon-lattice appears at higher binding energies rather than those of Srlattice, which is an important indicator for Sr-enrichment on the perovskite surface.45,46 Consequently, it was found that Srnon-lattice is ∼29%, far lower than Srlattice (∼71%), indicating that Sr segregation is not severe on the surface of BSCFZY. The aforementioned chemical compositions are summarized in Table S1.†
Other than BSCFZY, we prepared another type of self-assembled composite, Ba0.5Sr0.5Co0.6Fe0.2Ce0.1Y0.1O3−δ (BSCFCY) via Ce ion doping. Similar to Zr ions, the doping of Ce ions produced separated phases, as reflected in the XRD patterns (Fig. S8†). However, the Co contents over the grains are rather abruptly altered (see Fig. S9† for a detailed characterization), indicating that the Ce-rich phase is likely BaCexYyO3−δ. Given that barium cerates are proton-conducting ceramics, the BSCFCY composites appear to be auspicious when applied as a protonic ceramic fuel cell (PCFC) cathode rather than being applied as a SOFC cathode (Fig. S10†).
The viability of the developed composites as a PCFC cathode is additionally assessed, as parent BCFZY is a renowned cathode for PCFCs, and considerable attention has been directed at PCFCs recently due to their prospective performances at low temperatures. For this purpose, the half-cell with a symmetric configuration of BSCFZY|BaZr0.1Ce0.7Y0.1Yb0.1O3−δ (BZCYYb)|BSCFZY is tested. Fig. S16† shows the half-cell results of the BSCFZY cathode based on proton-conducting electrolytes. In this case, we found a low resistance value of ∼0.28 Ω cm2 at 650 °C, which indicates that BSCFZY is a promising cathode candidate for PCFCs as well. Significantly, the polarization resistance of BSCFZY decreases with an increase in the water vapor pressure (Fig. S16h†), implying that BSCFZY is capable of proton conduction and therefore functions as a triple-conducting (proton, oxygen vacancy and electron–hole) oxide.
Such a high performance outcome of BSCFZY is ascribed to the intimate networking of two individual nano-crystals, which enters a cooperative partnership (Fig. 5). Because both form a mixed-ionic-and-electronic conductor, the electrochemical reduction of oxygen is expected to occur over a significant portion of the electrode surface. However, the unique nano-network achieved in the form of the BSCFZY composite positively augments the ORR catalytic activity. For example, more electronically conductive Co-rich phases will aid adjacent Zr-rich phase by conducive electron–hole (h˙) transport, causing each and every part of the electrode to actively participate in the ORR. The Zr-rich phase, on the other hand, may effectively suppress the grain growth of the sinter-vulnerable Co-rich phase, hence fabricating a high-surface-area electrode that cannot be easily realized with conventional ceramic processing. In addition, Zr-rich phases can benefit stronger oxygen ion (O2−) conduction due to the larger lattice parameters (Table S2†).
Fig. 5 Schematic representation of possible oxygen electrochemical reduction pathways of self-assembled multi-phase cathodes with a synergistic ensemble effect. |
To determine whether the aforementioned discussions present reasonable points, a distribution of relaxation time (DRT) analysis of impedance spectroscopy is undertaken to determine possible rate-determining steps (Fig. 4c–e). The DRT analysis is a useful approach for understanding the reaction kinetics and transport phenomena of certain electrochemical systems based on the relaxation time differences among all the steps. For the ORR, the sub-processes can be largely classified into three groups: charge-transfer, surface exchange, and gas diffusion processes; Chen et al. proposed that each process can be attributed to the high-frequencies (HFs), mid-frequencies (MFs), and low-frequencies (LFs) of the impedance arc, respectively.8,16 The DRT of BSCFZY showed three distinct peaks, analogous to Chen's suggestion. A subsequent analysis based on the pO2 variance (0.05–1 atm, Fig. 4d and e) and temperature dependency (Fig. S17†) over DRT functions indicated that the above assignments are convincing. For example, the most pO2-dependent LF process is likely associated with gaseous oxygen mass transfer processes such as diffusion, as supported by the insignificant thermal activation (Fig. S17†).8,19,47 On the other hand, the least pO2-dependent HF process is possibly the charge transfer (O2−) across the electrode/electrolyte interface, and the remaining MF can be attributed to surface exchange processes, including the partial reduction of adsorbed oxygen and subsequent dissociation.48,49
We then compared the EIS and related DRT functions of BSCFZY to those of BSCF, BCFZY, and the ball-milled BSCF + BCFZY composite cathode (Fig. 6a and S18†), since the compositions of the phase isolated in BSCFZY (i.e., Co-BSCFZY and Zr-BSCFZY) are close enough to those of BSCF and BCFZY, respectively. The collective EIS and DRT analysis results here suggest that the Co-rich phase is responsible for facile HF and MF processes, while the Zr-rich phase promotes the LF processes, in the BSCFZY nanocomposite. For instance, it was found that the ORR rates of BSCF are considerably limited by the poor gas diffusion (Fig. 6c), in good agreement with the results of SEM (Fig. 6b). Indeed, when the microstructures of BSCF and BSCFZY were compared here, BSCFZY demonstrated an enhanced particle-sintering resistance as the particle size of BSCFZY is approximately four times smaller than that of BSCF. The small grain size found in BSCFZY composites can be helpful for facile gas diffusion (Fig. S19†). An additional Brunauer–Emmett–Teller (BET) analysis of the BSCFZY powder sample heat-treated at 1000 °C showed that the surface area is ∼1.68 m2 g−1, which is nearly one order of magnitude higher than that of BSCF (∼0.193 m2 g−1), providing further evidence that Zr-BSCFZY exhibits sinter-resistance.
A morphological comparison between BCFZY and BSCF found that the particle size of BCFZY was nearly two times smaller. Accordingly, in DRT analysis, BCFZY showed a weaker impact on the mass transfer resistance compared to the BSCF sample as expected from the refractory characteristics of this sample (Fig. 6d and S19†).33 However, the major polarization resistance of BCFZY prevails at the mid-frequency range, which is attributable to the limited electronic conductivity and thus the lack of ability to produce electronically charged oxygen intermediates at the surface. If the two cathode materials are physically mixed, the DRT functions show marginal improvements during both the MF and LF processes (Fig. 6e), whereas the most pronounced enhancements are only accomplished after BSCFZY self-assembles to form sub-microscale composites (Fig. 6f). The results indicate that the formation of an intimately dispersed nano-architecture as prompted from the self-assembly process is the key to achieve tailored characteristics favorable for the ORR process.
Surface exchange and bulk diffusion are closely related to the ORR rates as well. Accordingly, electrical conductivity relaxation is conducted between pO2 = 0.21 and 1 atm to measure the bulk diffusion coefficient (Dchem) and surface exchange coefficient (kchem) of BSCFZY (Fig. S20,† electronic conductivity of BSCFZY is shown in Fig. S21†). Significantly, the measured kchem values of BSCFZY are several orders of magnitude higher than those reported for BSCF and BCFZY samples. For instance, the reported kchem value at 450 °C for BCFZY is ∼1 × 10−4 cm s−1, and that for BSCF is ∼5 × 10−5 cm s−1, whereas the value observed for BSCFZY is ∼7.87 × 10−3 cm s−1, which is 78.7 and 157.4 times higher, respectively.27
To investigate in detail the reason for the performance enhancement in BSCFZY, O2 temperature-programmed-desorption (O2-TPD) tests were subsequently carried out in an effort to observe the dynamic process of oxygen adsorption and desorption on perovskite oxides of both BSCFZY and BSCF (Fig. S22†). To this end, the respective 100 mg powders were put under 50 ml min−1 He gas in the temperature range of 50–900 °C, with a ramping rate of 10 °C min−1. The resulting TCD signals were recorded using an AutoChem II 2920 device (Micromeritics).
O2-TPD provides useful information about oxygen mobility in oxides.27,50 Notably, perovskite oxides are known to desorb two types of oxygen ; the first is α-oxygen, which originates from the weakly adsorbed oxygen species on the surface in a relatively low-temperature region, and the second is β-oxygen, which originates from the tightly bonded lattice oxygen released at high temperatures.29,51 Accordingly, two distinctive peaks were readily identified in BSCFZY and BSCF. Notably, the BSCFZY composite shows the initial desorption temperature and peak temperature of α-oxygen at approximately 150 and 275 °C, respectively, lower than those in BSCF (186 and 279 °C). Significantly, the ratio of α-oxygen to β-oxygen (α-oxygen/β-oxygen) is found to be much higher in BSCFZY (BSCFZY: 1.95, BSCF: 0.33). This provides qualitative evidence for the faster surface oxygen exchange (kchem) found in BSCFZY due to the larger amounts of weakly bonded surface oxygen species available at the perovskite surface.
Additionally, the initial desorption temperature and peak temperature of β-oxygen found in the BSCFZY composite are approximately 470 and 594 °C, respectively, which are far lower than those in BSCF (500 and 710 °C). The faster activation of lattice oxygen in the bulk perovskite crystal may stem from the superior diffusivity (Dchem) found in the BSCFZY composite. Due to the substitution of Co3+ by the larger Zr4+ and Y3+ cations,52 the BSCFZY composite shows larger lattice parameters (Co-BSCFZY: 4.01 Å and Zr-BSCFZY: 4.13 Å) than BSCF (3.98 Å)53 and thus exhibits a larger free volume, commonly associated with increased oxygen mobility and decreased activation energy in perovskites.33,54 Accordingly, these results suggest the superior oxygen mobility in BSCFZY composites.
Next, the feasibility of the BSCFZY composite as a SOFC cathode is assessed though single cell tests. First, NiO-Gd0.1Ce0.9O2−δ (GDC10) powder is die-pressed to form anode pellets. After light sintering at 950 °C, the GDC20 electrolyte is sequentially deposited onto the anode support by a particle suspension coating process. This is followed by 1450 °C sintering for five hours, to prepare a Ni-GDC10|GDC20 anode-electrolyte bilayer. The cathode is then screen-printed onto the electrolyte and fired at 900 °C to complete the single-cell fabrication process. Fig. 7a shows a cross-sectional SEM image describing the microstructure of the single cell with a configuration of Ni-GDC10|GDC20|BSCFZY. The resulting cathode is approximately 30 μm thick, which is tightly bonded to the electrolyte (thickness: ∼13 μm), indicating good thermal compatibility between the BSCFZY cathode and the GDC20 electrolyte. Not surprisingly, the BSCFZY cathode reveals a nice cathode microstructure which consists of nano-sized grains (Fig. 7b), presumably due to the sinter-resistive characteristic originating from the Zr-BSCFZY phase. Fig. 7c shows typical I–V and I–P curves of button cells using H2 as the fuel and synthetic air as the oxidant. Accordingly, the cells delivered superior peak power density outcomes of ∼1.29 and 1.10 W cm−2 at 650 and 600 °C, highlighting the excellent outlook of the newly developed cathode achieved via the self-assembly process (the EIS of the single cell is measured and presented in Fig. S23†).
The long-term stability of the BSCFZY porous cathode was then assessed with another single cell based on the SDC electrolyte. The microstructure of the SDC-based single cell is similar to that of the GDC-based cell (Fig. 7d and e) but with a slightly thicker electrolyte layer (∼15 μm). The I–V characterization of the corresponding cell in the temperature range from 450 to 650 °C is shown in Fig. 7f (the EIS of the single cell is measured and presented in Fig. S24 and Table S3†). For an extended duration of ∼310 hours of operation under a constant voltage load of 0.7 V at 500 °C, the cell exhibited no noticeable degradation, indicating the exceptional stability provided by the nano-composite cathode (Fig. 7g).
While it is seldom reported, thermal cycling capability is also of paramount importance to ascertain for SOFCs to penetrate deeply into the market. Specifically, under accidental circumstances when the SOFC experiences a sudden temperature drop likely due to a shut-down event, or when a rapid start-up process is needed for an urgent power supply, wild thermal stress will be loaded onto the SOFC and the prevention of cell failure will crucially depend on the TEC mismatch between the cathode and the electrolyte. To test this, the cell here was put through five rapid ramping cycles between ∼400 and ∼600 °C with heating and cooling rates of ∼14 °C min−1 (Fig. 7h). Significantly, upon the completion of the cycling process, the cell fully recovered its performance capabilities, indicating the adequate thermomechanical compatibility of the BSCFZY cathode with the SDC electrolyte (Fig. 7i). In addition to the intrinsically low TEC value, here we presume that the self-assembly process forms in situ generated nanoscale interconnections with strong physical linking effects which may alleviate the expansion of the composite.41 In addition, the residual nano-pores could also serve to suppress the thermal stress, thereby facilitating an excellent thermomechanical compatibility with SOFC electrolytes.55,56 A chemical compatibility test between SDC and BSCFZY was further conducted via powder XRD by annealing the SDC-BSCFZY mixture powder at 600 °C for ten hours (Fig. S25†). The XRD profiles of the composite revealed that no secondary phase arose after high-temperature annealing, implying the reasonable chemical compatibility between electrolytes and developed cathodes.
Finally, we prepare a table of SOFC performance outcomes based on self-assembled composite cathodes to provide a clear comparison (Table S4†). The table shows that our work demonstrates the highest values ever reported, and along with their exceptional durability and thermal cycling capability, our new cathodes are highly promising for high-performance SOFCs to be operated at low-to-intermediate temperatures.
The as-synthesized BSCFZY nanopowder was electrodeposited on a Ni matrix using the process reported by Kim et al. for enabling APT analysis.57 APT measurements were conducted using a CAMECA LEAP 4000X HR instrument in a pulsed-laser mode at a pulse frequency of 100 kHz, laser pulse energy of 80 pJ, base temperature of 57 K, and evaporation rate of 0.003 atoms per pulse. Needle-shaped specimens for APT analysis were prepared with ultra-high resolution focused ion beam (Helios G4, FEI) using the standard lift-out protocol.58 APT data were analyzed using IVAS 3.8.4 software developed by CAMECA instruments.
Anode-supported single cells were prepared to conduct the fuel cell measurements. Anode powder of NiO, an electrolyte powder (SDC, GDC10 from Fuel cell materials), and starch at a weight ratio of 6:4:1 were initially ball-milled to obtain the anode substrate. The anode powders were pressed in a square steel die and pre-heated at 950 °C for one hour in ambient air to heat the fugitive pore-formers of the starch. Atop the anode substrate, the electrolyte slurry was drop-coated. The electrode slurry was prepared by suspending the electrolyte powders in an organic binder composed of polyvinylpyrrolidone (PVP, Alfa Aesar), butyl benzyl phthalate (Alfa Aesar), triethanolamine (Alfa Aesar), and terpineol (Alfa Aesar). The resulting anode|electrolyte bilayer was sintered at 1450 °C for five hours to densify the electrolyte. Finally, the electrode was screen-printed onto the electrolyte sides to complete the fabrication of the single cell. Two types of single cells (Ni-SDC|SDC|BSCFZY and Ni-GDC10|GDC20|BSCFZY) were used to demonstrate the fuel cell performance. The long-term stability measurements conducted here were based on the Ni-SDC|SDC|BSCFZY cell. Silver paste was used as the current collector.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ta08178k |
This journal is © The Royal Society of Chemistry 2022 |