Er3+-activated Ba2V2O7 upconversion nanosheets for dual-mode temperature sensing

Satish Kumar Samal , Sahana Kulkarni , Jyoti Yadav and Boddu S. Naidu *
Energy and Environment Unit, Institute of Nanoscience and Technology (INST), Mohali, Punjab 140306, India. E-mail: naidu245@gmail.com; sanyasinaidu@inst.ac.in

Received 15th December 2023 , Accepted 6th March 2024

First published on 7th March 2024


Abstract

So far, there has been substantial research on non-contact luminescence thermometry approaches that rely on luminescence intensity ratio (LIR) technology. However, there is limited availability of phosphors doped with Er3+ ions that exhibit on-par luminescence and high sensitivity. In this work, samples of Ba2V2O7:Er3+ were synthesized using a sol–gel method aided by citric acid. The luminescence properties of these samples, including upconversion and down-shifting, were investigated using both ultraviolet and 980 nm laser stimulation. When subjected to ultraviolet (UV) light, the sample exhibits a distinct broadband emission that appears pale green. This emission is a distinguishing property of the sample and is attributed to the presence of V2O72− ions. Upon being stimulated by a 980 nm laser, the sample exhibits standard green up-conversion Er3+ emission bands. Concurrently, an assessment was conducted on the phosphor's ability to measure temperature by analysing the LIR between the thermally coupled 2H11/2, 4S3/2 energy levels (TCELs) and the non-thermally coupled 2H11/2, 4F9/2 energy levels (NTCELs) of the Er3+ ion. The corresponding highest sensitivity of temperature for TCELs and NTCELs can position Ba2V2O7:Er3+ nanosheets as a capable option for materials utilized in temperature-sensing applications.


1. Introduction

Temperature measurement is critical in many fields, including healthcare, industry, research and technology. Temperature sensors have traditionally been used to monitor temperature; however, these sensors frequently need contact with the object being measured, making them inappropriate for some applications. But, with the introduction of optical thermometry, temperature measuring has become more flexible and precise. Optical thermometry is a non-contact method of measuring temperature that uses infrared (IR) radiation generated by an object to calculate its temperature. The increasing popularity of this technology may be attributed to its several benefits, including its high level of accuracy, extensive temperature range, rapid operation, and non-contact characteristics. These attributes make it well-suited for a broad range of applications across multiple sectors.1–3 Based on emission peak wavelength or peak width, luminescence intensity ratio (LIR), and lifetime of luminescence, various luminescent materials have been devised as temperature-sensing materials used in optical thermometers, of which those based on the LIR technique are widely used due to their ability to eliminate excitation source variation as well as fluorescence loss. The LIR approach capitalizes on the inconsistencies in the responses to temperature of two emission signals resulting from TCELs of transition metals or rare-earth (RE) ions that adhere to the Boltzmann population distribution.4–6 Due to the attractive optical features of visible light produced by near-IR excitation, many researchers have utilized the LIR technique to deal with RE ion-based upconversion (UC) emission signals.7–11 One of the most studied areas of LIR optical thermometers right now is the Er3+-doped system.12 Upon excitation at a wavelength of 980 nm, the numerous ladder-like energy levels of Er3+ may produce a bright green UC luminescence, which originates from the 2H11/24I15/2 and 4S3/24I15/2 transitions.13–16 High-quality LIR-based temperature sensing is made achievable by the exceptional thermal coupling between the 2H11/2 and 4S3/2 levels.17 The thermally coupled levels of Er3+ are separated by an energy gap of ∼800 cm−1, which falls in the ideal range of 200–2000 cm−1, in comparison to other lanthanide ions. Despite the extensive research on optical thermometers based on Er3+, there is still plenty of opportunity to enhance their thermometric sensitivity, detection range, and other critical performance parameters. Moreover, optical thermometers based on TCELs have low sensitivity since they are dependent on their energy difference (ΔE), which falls in the range of 200–2000 cm−1. Consequently, researchers are currently exploring the utilization of two separate NTCELs of RE ions in upconverting luminescent materials to address this limitation and enhance their temperature-sensing capacity.

Members of the vanadate-based phosphor group are good examples of materials with great thermal stability along with low phonon energy, allowing luminescence based on RE ions.18–20 The inclusion of the pyrovanadate group is an important benefit of Ba2V2O7-based phosphors over other vanadate or non-oxygen matrices, since they may exhibit exceptionally effective broadband luminescence in the visible light domain, making them suitable for use in lighting applications owing to their impressive color rendering capabilities.21 There are some reports on pyrovanadate-based nanomaterials that focus on their dielectric and luminescence properties as well as on their different synthesis routes.22–27 However, there is no approach towards their application in optical thermometers to date.

The present study utilized a citrate-assisted sol–gel technique to synthesize Er3+-doped Ba2V2O7-based (BVO) phosphors. The spectral properties of these as-synthesized phosphors were investigated under UV as well as NIR light. Temperature-dependent upconversion luminescence properties were studied, and also the possibility of their application for LIR-based dual-mode temperature sensing.

2. Experimental procedure

2.1. Chemicals required

Ba(NO3)2 (>99%) and V2O5 (>98%) were procured from Merck. Er(NO3)3·5H2O (>99.9%) was obtained from Thermo Scientific chemicals. Anhydrous citric acid (>99.5%) and concentrated HNO3 (∼69%) were purchased from Merck.

2.2. Synthesis of Ba2V2O7:Er3+ nanomaterials

A citrate-gel technique was used to synthesize BVO nanoparticles doped with x at.% Er3+ (x = 0.01–0.15). Stoichiometric quantities of Er(NO3)3, Ba(NO3)2, and V2O5 were weighed following the chemical formula and mixed in a beaker with 50 mL of aqua dest. To the above mixture, 2 mL of conc. HNO3 was added to facilitate the dissolution of V2O5. Subsequently, while maintaining a molar ratio of 2[thin space (1/6-em)]:[thin space (1/6-em)]1 between citrate and metal ions, a sufficient amount of citrate was introduced to the mixture in order to serve the role of chelating agent. Stirring was done at 363 K over a hot-plate stirrer until the formation of a wet gel (∼6 hours). The wet gel is then subjected to drying at 453 K for 12 hours. The resulting xerogel was ground in a mortar after being preheat-treated at 823 K for 5 hours. Finally, the white BVO powder was calcined for 3 hours at 1173 K before processing.

2.3. Characterization

A Bruker D8 Advance X-ray diffractometer was utilized to acquire X-ray diffraction (XRD) patterns. The purpose of these measurements was to examine the crystal phase of the powdered materials generated, within the scanning range of 10°–70°. The crystal structure viewing was done through VESTA software. The nanomaterials underwent morphological characterization by the utilization of a JEOL JSM-7610F Plus field-emission scanning electron microscope, which was aided by energy-dispersive X-ray spectroscopy (EDS). Specifically, a JEOL JEM 2100 Plus transmission electron microscope (200 keV, 0.14 nm resolution) was employed for this purpose. The experimental setup involved the utilization of an Agilent Cary 5000 spectrophotometer to obtain UV-visible-NIR diffuse reflectance spectra (DRS). The photoluminescence (PL) properties were examined using a Horiba Jobin–Yvon Fluorolog 3–221 fluorometer having a 450 W xenon lamp and a visible as well as an NIR photomultiplier tube (PMT) along with an external assembly consisting of a 980 nm CW laser diode.

For temperature-dependent PL experiments, 10 mg of the sample was mixed with a few drops of ethanol to make a slurry. For film formation, this slurry was further dropcast onto a quartz slide and left to dry under ambient conditions. This dropcast sample was used for PL measurements at temperatures ranging from 275 to 650 K using a VPF-800 Janis cryostat with a Lake Shore Model 335 temperature controller.

3. Results and discussion

3.1. Structural and morphological studies

To examine the impact of different concentrations of Er3+ dopant on the photoluminescence properties of this particular material, a series of nanoparticles with varied Er3+ concentrations ranging from 1 to 15 at% with respect to the Ba2+ ions were utilized. BVO:Er3+ nanoparticles crystallizing in the triclinic phase with a P[1 with combining macron](2) space group were generated because of the proposed easier approach. As is apparent in Fig. 1, all the diffraction reflections conform to the reference data (PDF 01-076-0612), with no extra peaks indicating the non-existence of another phase or by-products. A schematic of the Ba2V2O7 crystal structure is shown in Fig. S1 and the lattice parameters are shown in Table S1 of the ESI. With the increment in the concentration of Er3+, the lattice parameters decrease, leading to the conclusion that the Er3+ is substituting for the Ba2+ site, since Er3+ is smaller than Ba2+. The crystallite size of the as-prepared phosphors was calculated using the Scherrer equation.28 The computed crystallite size (D) of the nanomaterials falls within the range of 75–90 nm. High-resolution XPS spectra of undoped BVO and BVO:0.125 Er3+ samples demonstrate that oxygen vacancies are present in both the samples and their amount is higher in case of Er3+-doped samples, which show charge compensation due to the doping of Er3+ in the Ba2+ site (Fig. S2 of the ESI).
image file: d3nr06401h-f1.tif
Fig. 1 XRD patterns of Ba2V2O7 and its Er3+-doped nanomaterials.

In addition, the BVO host matrix as well as Er3+-doped BVO materials show sheet-like morphology as is evident from FE-SEM and TEM images displayed in Fig. 2(a and b). Fig. 2(c) exhibits the HR-TEM picture, which reveals distinct lattice fringes. The calculated d-spacing of 0.36 nm corresponds to the (002) main plane, providing conclusive evidence for the crystalline structure of the specimen. The dot pattern observed in the selective area electron diffraction (SAED) image (Fig. 2(d)) provides evidence that the particles under investigation possess a single structural phase. Fig. S3 of the ESI depicts the estimated composition of all the elements present in undoped BVO as per EDS and the mapping of elements, which convey and verify the consistent dispersal of constituent elements throughout the analysed sample.


image file: d3nr06401h-f2.tif
Fig. 2 (a) Field-emission SEM, (b) TEM, (c) HR-TEM, and (d) electron (SAED) diffraction images of undoped Ba2V2O7 sheets.

3.2. Optical properties

DRS spectra of undoped and Er3+-doped Ba2V2O7 nanosheets are recorded in the UV-visible-NIR region and presented in Fig. 3. The undoped sample shows broad absorption in the UV range, spanning from 200 to 400 nm with two shoulders. This is attributed to the optical absorption of the vanadate group due to ligand-to-metal charge transfer (LMCT), and can be explained by the charge transfer from O2− 2p orbitals to V5+ 3d orbitals in the tetrahedral VO43− symmetry group. This absorption is frequently linked to the transfer of excited electrons from the ground state (GS) 1A1 to the excited states (ES) 1T1,2.25,29 In Er3+-doped samples, apart from the host absorption bands, several sharp peaks in the range from 375–1600 nm are observed, which correspond to the 4f–4f Er3+ transitions, i.e. absorption from the 4I15/2 ground state to 4I13/2 (1531 nm), 4I11/2 (976 nm), 4I9/2 (797 nm), 4F9/2 (653 nm), 4S3/2 (546 nm), 2H11/2 (520 nm), 4F7/2 (480 nm), 4F5/2 (450 nm) and 4G11/2 (380 nm) excited states. The designation of optical absorption bands is based on previous findings.30
image file: d3nr06401h-f3.tif
Fig. 3 UV-visible-NIR DRS of Ba2V2O7:xEr3+ nanomaterials.

3.3. Photoluminescence properties

Fig. 4(a) displays the photoluminescence excitation (PLE) spectrum of the BVO host material in the range of 275–400 nm and it has been further deconvoluted using a Gaussian fitting. The spectrum displayed distinct deconvoluted excitation peaks, positioned around 290 and 347 nm. In vanadate compounds, the excitation broadband is typically dictated by the host lattice structure and the vanadate concentration.31 The deconvoluted excitation spectrum denoted as Ex1, which is located at a wavelength of 290 nm, is associated with the spin-allowed transition from the 1A1 to the 1T2 electronic state. On the other hand, at the higher excitation band of 347 nm, referred to as Ex2, is assigned the spin-permitted electronic transition from the 1A1 to the 1T1 state.22 The electrons in the 1T1 and 1T2 states decay non-radiatively to 3T1 and 3T2 states, from where they decay radiatively to the 1A1 by emitting a very broad emission spanning the wavelength range of 375–675 nm as shown in Fig. 4(b). The O2− → V5+ charge transfer (CT) is responsible for this broadband emission.32–34 The difference in energy between the 3T1 and the 3T2 excited state is ∼0.3 eV, which means that the two broad peaks overlap and cannot be differentiated from one another. Hence the broad band is deconvoluted into two bands. The compact band (Em1) at the shorter wavelength positioned at 495 nm refers to the 3T21A1 electronic transition, while the somewhat larger band (Em2) is imputed to the 3T11A1 electronic transition of the vanadate group, with the band maximum detected at 567 nm (inset of Fig. 4(a)). The relative FWHM values of the Em1 and Em2 bands were determined to be 110 and 164 nm, respectively.
image file: d3nr06401h-f4.tif
Fig. 4 Gaussian deconvoluted photoluminescence excitation spectra (a) and emission spectra (b) of undoped Ba2V2O7 with the inset in (a) depicting the schematic transition processes in the vanadate.

To comment on the genesis of luminescence in vanadates, as reported previously, CT in vanadate with Td symmetry is the cause.32,35 In general, the 1A11T1,2 excitation process is permitted in the ideal Td symmetry, but the spin selection rule prohibits the 1T1,23T1,2 intersystem crossing, as well as 3T1,21A1 luminescence processes. In spite of this, the structure of the VO4 tetrahedron is not identical to that of an ideal tetrahedron. This is because corner-sharing VO4 dimers induce major distortions in the structure of the VO4 tetrahedron. As a result, previously disallowed processes are now partially permitted owing to the spin–orbit interaction.

The incorporation of dopants, namely Er3+ ions, as seen in Fig. 5(a–d), induces small changes in both the emission profile and intensity of the 513 nm emission spectrum over the series. This phenomenon may be attributed to the sensitivity of Er3+ to UV light, resulting in the observation of several energy dips associated with Er3+ transitions: 4F7/24I15/2 (488 nm), 2H11/24I15/2 (524 nm, G1 peak), and 4S3/24I15/2 (545 nm, G2 peak). Moreover, when the concentration of Er3+ increases, the intensity of certain transitions is enhanced due to the improved energy transfer (ET) efficiency between [V2O7]4− and Er3+. This is evident in Fig. 5(a) where the host emission profile diminishes and the Er3+ emission intensity, as shown in Fig. 5(c), rises with an increase in dopant concentration. The sample doped with x = 0.125 Er3+, on the other hand, has the maximum luminescence intensity. After x = 0.125, the luminescence intensity decreases, which can be ascribed to concentration quenching based on inter-4f cross relaxations. Fig. S4 of the ESI illustrates contour graphs representing the emission and excitation characteristics of Ba2V2O7:Er3+ nanomaterials. This resource offers qualitative data on potential excitation wavelengths and the corresponding emission intensities. This observation highlights the significant impact of the excitation wavelength on the relative emission intensities within the visible region.


image file: d3nr06401h-f5.tif
Fig. 5 Photoluminescence spectra excited at (a) 345 nm and (c) 488 nm in the visible region, (e) 345 nm in the NIR region, and excitation spectra monitored at (b) 513 nm, (d) 556 nm, and (f) 1541 nm emission of Ba2V2O7:xEr3+ (x = 0–0.15).

In addition to examining spectra within the visible range, the emission of the samples doped with erbium was assessed in the near-infrared (NIR) area (Fig. 5(e and f)). The observation of Er3+ NIR emission with a 1541 nm peak signifies the involvement of ET from BVO to Er3+ ions. Fig. 5(e) displays the NIR emission spectra obtained from Er3+-doped Ba2V2O7 nanoparticles when stimulated at 345 nm. There exists a band that is notable for its distinctiveness and is finely split due to the transitions at 4I13/24I15/2 (1541 nm). The intensity exhibits an upward trend with increasing concentrations of Er3+ up to a threshold of 0.125, beyond which it steadily decreases. The phenomenon of concentration quenching is accountable for the reduction in emission intensity observed above the threshold value of x = 0.125. The transfer of energy to the Er3+ ion leads to several 4f–4f transitions occurring in the visible as well as NIR regions. However, the diminished intensity of absorption by the host material indicates this phenomenon.

The ET from BVO to Er3+ ions can also be elucidated by analysis of the decay lifetime of the 513 nm host emission (λex = 345 nm) (Fig. S5 of ESI). The bi-exponential decay function provided below effectively modeled the decay curve of the host lattice:

 
image file: d3nr06401h-t1.tif(1)

The variable I(t) denotes the count at time ‘t’. The constants τ1 and τ2 correspond to the decay lifetime. The average lifetime value may be determined by utilizing the following equation:

 
image file: d3nr06401h-t2.tif(2)

The average lifetime values of the Er3+-doped Ba2V2O7 phosphor are tabulated in Table S2 of the ESI. The decay lifetime of the host lattice can be accurately described by a bi-exponential function. The slower decay observed in this function is attributed to the ET between V2O72− and the Er3+ dopant. On the other hand, the quicker kinetics observed may be attributed to the surface interaction on the BVO material. When increasing the Er3+ concentration in the host lattice, the average lifetime values decrease, which can be attributed to the enhanced energy transfer occurring from the host to Er3+ ions. The energy transfer efficiency (ηET) is calculated from the host emission in the presence and absence of Er3+ ions and is illustrated in Fig. S6 of the ESI. It increases when increasing the dopant concentration and reaches a maximum of 52% for the BVO:0.15Er3+ sample.

For an examination of the luminescence characteristics of BVO:xEr3+ in the process of upconversion, the samples were subjected to illumination using a 980 nm laser diode with a power density of 0.041 W mm−2. The resulting emission spectrum was recorded and is presented in Fig. 6(a). The optimization of luminescence properties is achieved by the manipulation of the percentage of dopant ions (ranging from x = 0.02–0.15) inside the Ba2V2O7 host matrix. The emission intensity demonstrates an upward trend as the amount of Er3+ ions increases, reaching its peak at x = 0.125, as is evident from the visible and NIR emission spectra, and which is considered the optimal concentration. Subsequently, the emission intensity declines. The observed phenomenon can be ascribed to concentration quenching, namely the heightened inter-Er3+ cross-relaxation. The spectral analysis of the UC (upconversion) phenomenon reveals prominent peaks in the green area of the electromagnetic spectrum, namely at wavelengths of 524 nm and 545 nm. These peaks may be imputed to the 2H11/2 and 4S3/24I15/2 transitions of Erbium ions, respectively, which are classified as 4f–4f transitions.


image file: d3nr06401h-f6.tif
Fig. 6 (a) Upconversion luminescence of doped Ba2V2O7:xEr3+ phosphors upon excitation with a 980 nm laser. (b) Laser power-dependent upconversion luminescence of Ba2V2O7:0.125Er3+. (c) Plot of ln(I) vs. ln(P) of Ba2V2O7:0.125Er3+.

To evaluate the process of UC emission, a mono-log plot was conducted by varying the pump power density to examine the connection between upconversion intensity and pump power, as shown in Fig. 6(b and c). This analysis was based on the non-linear relationship expressed as,

 
Intensity ∝ Pump powern.(3)

In the context of the UC mechanism, the variable ‘n’ denotes the quantity of pump (NIR) photons participating in the process. The slope values for emission at 524 nm and 545 nm were determined as 1.85 and 2.32, respectively, by an investigation of the pump power dependency of the BVO:0.125Er3+ phosphor (see Fig. 6(c)). Based on the observation that the value of ‘n’ just exceeds 2, it may be inferred that the emission in the green area of BVO:Er3+ phosphors is attributed to a 2-photon UC mechanism. For the 407 nm blue emission, even though the value of ‘n’ is not close to 3, the presence of a 407 nm peak upon excitation with a 980 nm laser, shown in Fig. S7 of the ESI, is only possible when a 3rd photon governs the UC process, which is explained later on in the section. In addition to the effect of pump power density on the intensity of the sample, it affects the internal temperature of the phosphor. This is known as laser heating and the same phenomenon has been mentioned in Fig. S8 of the ESI.

The energy level diagram depicted in Fig. 7 serves as a visual representation of the hypothetical 980 nm stimulated UC luminescence mechanism seen in erbium-doped barium vanadate (BVO). The primary processes identified as being responsible for the emission of UC include ground and/or excited-state absorption, as well as non-radiative relaxations (NR). The process of single-photon absorption facilitates the transfer of population from the GS 4I15/2 to the ES 4I9/2. Conversely, two-photon absorption via resonance allows the population to be moved to the 4F7/2 excited state. There are three lower excited states that the 2H9/2 species can spontaneously decay to: 2H11/2, 4S3/2, and 4F9/2. The process of relaxation is accompanied by emission in the green and red spectral regions. The ions inhabiting the ES 4I9/2 experience NR relaxation towards the lower ES 4I11/2 and 4I13/2, leading to the 1541 nm emission. The presence of a third photon can be detected throughout the excitation process from the lower 4F9/2 level to the higher 2H9/2 level. This excitation results in the subsequent emission of light at a wavelength of 407 nm, as well as further non-radiative relaxations down to the lower energy levels.


image file: d3nr06401h-f7.tif
Fig. 7 Schematic of the energy levels of Er3+-doped Ba2V2O7, showing the potential transition mechanism.

3.4. Temperature-sensing studies

Fig. 8(a) illustrates the upconversion spectra of BVO:0.125Er3+ at different temperatures when subjected to 980 nm laser irradiation at a power density of 0.041 W mm−2. The temperature investigated spans from 275 to 650 K, the intention being to examine the optical thermometry of rare earth (RE) luminescence. The empirical evidence indicates that the intensity profile of the G1 and G2 peaks exhibits a reduction as the temperature increases, but the placements of the bands stay constant. The intensity of the G2 band, which arises from the 4S3/2 energy level, exhibits a decline as temperature increases. Moreover, this decline occurs at a faster rate compared to the intensity drop observed in the red emission (4F9/24I15/2, denoted by R). The phenomenon of thermal quenching is seen due to the NR relaxation from the 4S3/2 to 4F9/2 levels. As a result of this process, the number of electrons in the 4F9/2 level rises while the number of electrons in the 4S3/2 level falls. Another factor to consider is the effective utilization of heat activation in promoting the transition of electrons from the 4S3/2 to the 2H11/2 energy level. As an outcome, the strength of the emission signal from the 4S3/2 level is diminished. Fig. 8(b) shows that when temperatures rise, the G1/G2 ratio rises. This is because the TCELs and thermal agitation have a small energy gap, thus, the G1 emission is stronger at higher temperatures.
image file: d3nr06401h-f8.tif
Fig. 8 Temperature-varied (a) UC PL spectra and (b) 551 nm normalized emission spectra of Ba2V2O7:0.125Er3+.

Fig. 9 and 10 illustrate the graphical representation of the two typical LIR techniques for BVO:0.125Er3+ (G1/G2 and G1/R) with respect to temperature. The LIR of TCELs may be described by a Boltzmann distribution:36

 
LIR = B[thin space (1/6-em)]exp(−C/T)(4)


image file: d3nr06401h-f9.tif
Fig. 9 (a) Temperature dependence of emission intensity ratio and (b) corresponding sensitivities for TCELs of Ba2V2O7:0.125Er3+.

image file: d3nr06401h-f10.tif
Fig. 10 (a) Temperature dependent luminescence intensity ratio and (b) corresponding sensitivities for NTCELs of Ba2V2O7:0.125Er3+.

In the above eqn (4), B is denoted as a constant. The variable C is determined by dividing the energy difference (ΔE) by the Boltzmann value (kB), while T denotes the temperature in Kelvin. The absolute (Sa) and relative (Sr) sensitivities are further derived from the above equation:

 
image file: d3nr06401h-t3.tif(5)
 
image file: d3nr06401h-t4.tif(6)
]Fig. 9(b) displays the variation of Sa and Sr as a function of temperature. At temperatures of 550 K and 275 K, the observed maxima for Sa and Sr are determined as 0.0026 K−1 and 1.40% K−1, respectively.

The levels, 2H11/2 and 4F9/2, are classified as non-thermally coupled energy levels (NTCELs) due to their significant disparity in energy levels, which prevents them from achieving thermal equilibrium. The temperature dependency of the spectral intensity variation in the R band is clearly demonstrated as being identical to that in the G2 band (see Fig. 8(b)). Consequently, the performance of temperature measurements utilizing the LIR properties of the 2H11/2 and 4F9/2 energy levels is evaluated. The equation provided can be used to fit the FIR values of the NTCELs (G1/R):

 
LIR = B1 + B2T + B3T2 + B4T3(7)
where Bn, n = 1, 2, 3, 4 denotes the fitting constant of the polynomial.37 The LIR function for the NTCELs in the temperature range of 275–650 K is shown in Fig. 10(a). The absolute and relative sensitivities associated with this function are computed using the aforementioned expression:
 
image file: d3nr06401h-t5.tif(8)
 
image file: d3nr06401h-t6.tif(9)

When the temperature increases, Sr falls, while Sa first rises and subsequently falls. The highest values of Sa and Sr are seen at 350 K and 275 K, respectively, with magnitudes of 0.023 K−1 and 0.54% K−1, as depicted in Fig. 10(b).

Luminescent thermometric materials should have a wide temperature range to maximize their application, since this is a key feature of these materials. But in general, the intensity of emission of phosphors diminishes with rising temperature owing to thermal quenching. Consequently, their use in thermometry devices results in significant performance drops when exposed to high temperatures. In correspondence to this, Table 1 presents a comparative analysis of the temperature characteristics shown by several temperature-sensitive materials in various temperature ranges, mostly until 573 K. As is evident, the BVO:0.125Er3+ phosphor has good sensitivity in the higher temperature range (until 650 K). With reference to Table 1, the sensitivity shown by the Er3+ single-doped phosphor is comparable to or even better than that of the Yb3+, Er3+/Ho3+ codoped phosphors.

Table 1 Temperature-sensing characteristics of different upconversion materials
Compounds Temperature range (K) S a (10−4 K−1) S r (% K−1) Ref.
BVO:0.125Er (2H11/2/4S3/2) 275–650 26 1.40 This work
BVO:0.125Er (2H11/2/4F9/2) 275–650 230 0.54 This work
KBi(MoO4)2:Yb/Er 200–550 123 1.82 38
YVO4:Yb/Er 300–485 116.9 0.86 39
NaY2F7:Yb/Er 323–563 36 1.00 40
BaGdF5:Er 300–720 21 1.36 41
LuVO4:Yb/Er@SiO2 NPs 303–353 115 1.07 42
BaMoO4:Yb/Er 293–553 46 1.08 43
Sc2Mo3O12:Ho/Yb 303–573 275 44
Ca2MgWO6:Yb/Er 303–573 82 0.92 45
Bi5IO7:Er 303–543 69 1.36 46
KBaY(MoO4)3:Yb3+,Er3+ 250–460 130.6 1.80 47
KBaY(MoO4)3:Yb3+,Ho3+ 53–293 186 31.45 48


4. Conclusion

In conclusion, this study represents the first investigation into the thermometric characteristics of BVO:Er3+ samples exhibiting favorable upconversion (UC) emission. Triclinic BVO sheet-like nanophosphors are prepared by a citrate-gel technique. The samples exhibit excellent downshifting and upconversion luminescence upon illumination with a UV-vis lamp and 980 nm laser, respectively. The elucidation of the energy level diagram shows that the upconversion process involves a 2-photon mechanism. In the present study, an investigation was conducted on the temperature-sensing capabilities of the LIR technology utilizing the TCELs and NTCELs of Er3+ ions. The findings indicated that the highest temperature sensitivity attained was 1.40% K−1 and 0.54% K−1, respectively. Due to its enhanced UC luminescence and temperature-sensing characteristics, the synthesized phosphor exhibits potential as a viable option for optical thermometry applications.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

BSN thanks the DST-SERB, India, for financial support (grant no. CRG/2021/007668); CSIR India (JY), and INST Mohali (SKS) are acknowledged for their Fellowships.

References

  1. A. K. Singh, S. K. Singh, B. K. Gupta, R. Prakash and S. B. Rai, Dalton Trans., 2012, 42, 1065–1072 RSC .
  2. A. D. Pickel, A. Teitelboim, E. M. Chan, N. J. Borys, P. J. Schuck and C. Dames, Nat. Commun., 2018, 9, 4907 CrossRef PubMed .
  3. L. Marciniak, K. Elzbieciak-Piecka, K. Kniec and A. Bednarkiewicz, J. Chem. Eng., 2020, 388, 124347 CrossRef CAS .
  4. A. C. Brandão-Silva, M. A. Gomes, Z. S. Macedo, J. F. M. Avila, J. J. Rodrigues and M. A. R. C. Alencar, J. Phys. Chem. C, 2018, 122, 20459–20468 CrossRef .
  5. O. A. Savchuk, J. J. Carvajal, C. Cascales, M. Aguiló and F. Díaz, ACS Appl. Mater. Interfaces, 2016, 8, 7266–7273 CrossRef CAS PubMed .
  6. Y. Tian, B. Tian, C. Cui, P. Huang, L. Wang and B. Chen, RSC Adv., 2015, 5, 14123–14128 RSC .
  7. G. Chen, R. Lei, F. Huang, H. Wang, S. Zhao and S. Xu, Opt. Commun., 2018, 407, 57–62 CrossRef CAS .
  8. H. Lu, H. Hao, Y. Gao, D. Li, G. Shi, Y. Song, Y. Wang and X. Zhang, Microchim. Acta, 2017, 184, 641–646 CrossRef CAS .
  9. Z. Cheng, M. Meng, J. Wang, Z. Li, J. He, H. Liang, X. Qiao, Y. Liu and J. Ou, Nanoscale, 2023, 15, 11179–11189 RSC .
  10. J. D. Kilbane, E. M. Chan, C. Monachon, N. J. Borys, E. S. Levy, A. D. Pickel, J. J. Urban, P. J. Schuck and C. Dames, Nanoscale, 2016, 8, 11611–11616 RSC .
  11. O. A. Savchuk, J. J. Carvajal, C. D. S. Brites, L. D. Carlos, M. Aguilo and F. Diaz, Nanoscale, 2018, 10, 6602 RSC .
  12. H. Suo, X. Zhao, Z. Zhang, R. Shi, Y. Wu, J. Xiang and C. Guo, Nanoscale, 2018, 10, 9245–9251 RSC .
  13. K. C. Liu, Z. Y. Zhang, C. X. Shan, Z. Q. Feng, J. S. Li, C. L. Song, Y. N. Bao, X. H. Qi and B. Dong, Light: Sci. Appl., 2016, 5, e16136 CrossRef CAS PubMed .
  14. J. Zhang, Z. Hao, J. Li, X. Zhang, Y. Luo and G. Pan, Light: Sci. Appl., 2015, 4, 239 CrossRef .
  15. B. Dong, D. P. Liu, X. J. Wang, T. Yang, S. M. Miao and C. R. Li, Appl. Phys. Lett., 2007, 90, 181117 CrossRef .
  16. X. Bai, H. Song, G. Pan, Y. Lei, T. Wang, X. Ren, S. Lu, B. Dong, Q. Dai and L. Fan, J. Phys. Chem. C, 2007, 111, 13611–13617 CrossRef CAS .
  17. X. Wang, Q. Liu, Y. Bu, C.-S. Liu, T. Liu and X. Yan, RSC Adv., 2015, 5, 86219–86236 RSC .
  18. N. Kaczorowska, A. Szczeszak and S. Lis, Ceram. Int., 2021, 47, 24182–24190 CrossRef CAS .
  19. Y. Tian, J. Solid State Light., 2014, 1, 1–15 CrossRef .
  20. Y. Baoxiang, H. Jinyong, Z. Guifang and G. Jike, Vanadium, 2021, 395–413 Search PubMed .
  21. R. Yu, N. Xue, S. Huo, J. Li and J. Wang, RSC Adv., 2015, 5, 63502–63512 RSC .
  22. T. Nakajima, M. Isobe, T. Tsuchiya, Y. Ueda and T. Manabe, Opt. Mater., 2010, 32, 1618–1621 CrossRef CAS .
  23. M. R. Joung, J. S. Kim, M. E. Song, S. Nahm and J. H. Paik, J. Am. Ceram. Soc., 2009, 92, 3092–3094 CrossRef CAS .
  24. A. Sharma, M. Varshney, K. H. Chae and S. O. Won, RSC Adv., 2018, 8, 26423–26431 RSC .
  25. M. Takahashi, M. Hagiwara and S. Fujihara, Inorg. Chem., 2016, 55, 7879–7885 CrossRef CAS PubMed .
  26. N. V. Bharathi, T. Jeyakumaran, S. Ramaswamy and S. S. Jayabalakrishnan, Mater. Res. Express, 2019, 6, 106202 CrossRef .
  27. N. Kaczorowska, A. Szczeszak, W. Nowicki and S. Lis, Polyhedron, 2022, 223, 115940 CrossRef CAS .
  28. B. D. Cullity, Elements of x-ray diffraction, Addison-Wesley Publishing Company, Inc., 1978 Search PubMed .
  29. R. Yu, M. Yuan, T. Li, Q. Tu and J. Wang, RSC Adv., 2016, 6, 90711–90717 RSC .
  30. W. T. Carnall, P. R. Fields and K. Rajnak, J. Chem. Phys., 2003, 49, 4424 CrossRef .
  31. E. Pavitra, G. S. R. Raju, J. Y. Park, L. Wang, B. K. Moon and J. S. Yu, Sci. Rep., 2015, 5, 1–13 Search PubMed .
  32. H. Ronde and G. Blasse, J. Inorg. Nucl. Chem., 1978, 40, 215–219 CrossRef CAS .
  33. K. C. Park and S.-I. Mho, J. Lumin., 2007, 122–123, 95–98 CrossRef CAS .
  34. S. Benmokhtar, A. El Jazouli, J. P. Chaminade, P. Gravereau, F. Guillen and D. De Waal, J. Solid State Chem., 2004, 177, 4175–4182 CrossRef CAS .
  35. T. Nakajima, M. Isobe, T. Tsuchiya, Y. Ueda and T. Manabe, J. Phys. Chem. C, 2010, 114, 5160–5167 CrossRef CAS .
  36. L. H. Fischer, G. S. Harms and O. S. Wolfbeis, Angew. Chem., Int. Ed., 2011, 50, 4546–4551 CrossRef CAS PubMed .
  37. Z. Zheng, J. Zhang, X. Liu, R. Wei, F. Hu and H. Guo, Ceram. Int., 2020, 46, 6154–6159 CrossRef CAS .
  38. S. K. Samal, J. Yadav and B. S. Naidu, Ceram. Int., 2023, 49, 20051–20060 CrossRef .
  39. M. K. Mahata, K. Kumar and V. K. Rai, Sens. Actuators, B, 2015, 209, 775–780 CrossRef CAS .
  40. H. L. Gong, X. S. Peng, G. A. Ashraf, F. F. Hu, R. F. Wei and H. Guo, Ceram. Int., 2022, 48, 4023–4030 CrossRef CAS .
  41. F. Hu, S. Lu, Y. Jiang, R. Wei, H. Guo and M. Yin, J. Lumin., 2020, 220, 116971 CrossRef CAS .
  42. G. Xiang, X. Liu, J. Zhang, Z. Liu, W. Liu, Y. Ma, S. Jiang, X. Tang, X. Zhou, L. Li and Y. Jin, Inorg. Chem., 2019, 58, 8245–8252 CrossRef CAS PubMed .
  43. R. Lei, X. Liu, F. Huang, D. Deng, S. Zhao, H. Xu and S. Xu, Opt. Mater., 2018, 86, 278–285 CrossRef CAS .
  44. H. Zou, B. Chen, Y. Hu, Q. Zhang, X. Wang and F. Wang, J. Phys. Chem. Lett., 2020, 11, 3020–3024 CrossRef CAS PubMed .
  45. Y. C. Jiang, Y. Tong, S. Y. Z. Chen, W. N. Zhang, F. F. Hu, R. F. Wei and H. Guo, J. Chem. Eng., 2021, 413, 127470 CrossRef CAS .
  46. L. Luo, W. Ran, P. Du, W. Li and D. Wang, Adv. Mater. Interfaces, 2020, 7, 1902208 CrossRef CAS .
  47. K. Li, D. Zhu and H. Lian, J. Alloys Compd., 2020, 816, 152554 CrossRef CAS .
  48. K. Li, D. Zhu and C. Yue, J. Mater. Chem. C, 2022, 10, 6603–6610 RSC .

Footnote

Electronic supplementary information (ESI) available: Crystal structure, elemental mapping, O 1s photoelectron spectra, emission–excitation contour plots, and photoluminescence spectra in the visible region, energy transfer efficiency, excited state decay curves, as well as lattice parameters and lifetime values. See DOI: https://doi.org/10.1039/d3nr06401h

This journal is © The Royal Society of Chemistry 2024
Click here to see how this site uses Cookies. View our privacy policy here.