Herein, we carried out first-principles calculations based on density functional theory to investigate the effects of surface functionalization with hydrogen atoms on structural, dynamical and electronic properties of Cu2Si monolayer. Pristine Cu2Si, a metallic monolayer, has a planar hexacoordinate structure. Calculations revealed that the most favorable position of a single H atom on the Cu2Si monolayer is at the top of a Si site. Derivatives of Cu2Si monolayer with various H concentrations were investigated, and by performing phonon calculations, it was found that there are three stable hydrogenated structures. Specific heat of these monolayers was found to increase with the hydrogen concentration at temperatures higher than 100 K. Electronically, the hydrogenated derivatives of Cu2Si monolayer preserve the metallic character.
One of these novel materials is the monolayer Cu2Si15 with planar hexacoordinated Cu and Si motifs. It is a nonmagnetic metal with high stability stemming from the superposition of 4c–2e σ bonds extended within the 2D sheet. The metallicity of Cu2Si has been known, Feng et al. verified Dirac nodal line fermions in Cu2Si monolayer by using angle-resolved photoemission spectroscopy and first-principles calculations.16 Nodal line semimetals,17,18 a type of topological semimetals, have symmetry-protected linear-band crossing points near the Fermi level and they have been intensively studied previously.19 These materials are suitable candidates for the realization of high-speed, low-dissipation devices.16
Chemical functionalization of 2D materials is one of the most common methods to tune the structural,20 electronic21 and magnetic22 properties of a material. For instance, H and F atoms are commonly used for the surface functionalization of the 2D materials. Following the theoretical prediction of hydrogenated graphene (graphene),23 Elias et al. achieved the synthesis of the graphene and showed that the reversible hydrogenation process changes graphene into an insulator.24 Moreover, Nair et al. achieved to synthesize fluorinated graphene (fluorographene) which possesses completely different electronic properties than that of graphene.25 Although graphene is a highly conductive semimetal, fluorographene is an insulator with an optical gap of 3 eV. Recently, we reported that when the charge density wave (CDW) phase of single-layer TiSe2 is fully hydrogenated, the structure transforms to a distorted T-phase (Td).26 In the mean time, hydrogenation is also used for the passivation of interfaces and contacts.27,28 For instance, electrical conductivity of metals can be changed through various manipulations such as binding foreign molecules or adatoms.29 During experiments, the presence of the environmental interactions is inevitable; therefore, the passivation of such materials plays important role in achieving a stable electrical behavior. When the material is hydrogenated, the hydrogen layer acts as a protective layer against the external influences while preserving the electronic properties of the structure.
Even though there are several analyses on structural, chemical and electronic properties of the Cu2Si, the effect of hydrogenation has not been studied thoroughly. Herein, we present an investigation of the feasibility of the hydrogenation of the Cu2Si monolayer based on density-functional theory. Starting from single atom adsorption, structural, electronic and vibrational properties of Cu2Si covered with various concentrations of hydrogen are investigated. Three possible structures of hydrogenated Cu2Si are found to be dynamically stable. As well as the pristine structure, hydrogenated derivatives of Cu2Si monolayer exhibit metallic behavior. Moreover, it is found that the hydrogenation of Cu2Si monolayer leads to an increase in its specific heat at temperatures higher than 100 K and it reduces the surface activity of the material against other foreign agents without effecting its metallic character and planar geometry.
The paper is organized as follows: detailed information about computational methodology is given in Sec. II. The structural, vibrational and electronic properties of pristine Cu2Si, and also the adsorption and diffusion of a hydrogen atom on Cu2Si are discussed in Sec. III. In Sec. IV, we present the structural, vibrational and electronic properties of the hydrogenated derivatives of Cu2Si monolayer. Lastly, Sec. V is allocated for the conclusions.
Energy cutoff of the plane-wave basis set was chosen to be 500 eV. For the convergence criterion, the energy difference between successive electronic steps was taken to be 10−5 eV and the Hellmann–Feynman forces on each atom were reduced to a value of less than 10−4 eV Å−1. A vacuum space of 12 Å was incorporated in order to avoid the interactions between the adjacent layers. 18 × 18 × 1 Γ-centered mesh was used for the Brillouin Zone (BZ) integration of the unit cell and the mesh is scaled accordingly for larger supercells.
Cohesive energy per atom (Ecoh) was calculated for each structure, by using the following formula,
(1) |
a (Å) | b (Å) | γ (°) | dCu–Si (Å) | dCu–Cu (Å) | Δρ (e) | Ecoh (eV per atom) | |
---|---|---|---|---|---|---|---|
Cu2Si | 4.10 | 4.10 | 60.0 | 2.37 | 2.37 | 0.2 | 3.55 |
LowH-d | 8.09 | 8.09 | 58.4 | 2.33–2.44 | 2.34–2.46 | 0.4 | 3.57 |
HighH-s | 4.12 | 4.12 | 60.0 | 2.41 | 2.38 | 0.6 | 3.59 |
HighH-d | 8.21 | 8.27 | 59.7 | 2.41–2.42 | 2.38 | 0.6 | 3.59 |
In order to investigate dynamical stability, phonon band dispersion of the Cu2Si monolayer is calculated and is shown in Fig. 1(b). A 5 × 5 × 1 supercell is used for the phonon band structure calculations and it is found that the Cu2Si monolayer is dynamically stable. As seen in the figure, the signature of a Kohn-type soft phonon mode appears at the M point in the BZ.38 The highest-frequency modes, longitudinal optical (LO) modes, are mainly composed of the in-plane motions of Si atoms. The transverse optical (TO) modes that represent the out of phase vibrations of Cu atoms, have lower frequencies than that of the LO modes. Fig. 1(b) shows that Cu2Si monolayer has 2 optical flexural (ZO) modes. While the low-frequency mode is composed of out-of-plane motions of Cu atoms in opposite direction, the other mode consists of counter-phase motions of Cu and Si atoms in the out-of-plane direction. Compared to the typical 2D materials such as graphene (∼1500 cm−1),39 h-BN (∼1600 cm−1)40 and MoS2 (∼480 cm−1),41 phonon modes of the Cu2Si monolayer reside at lower energies.
Fig. 1(c) illustrates the electronic band dispersion and the partial density of states (PDOS) of the Cu2Si monolayer. As can be seen in the figure, the Cu2Si monolayer is a metal and exhibits nodal lines around the Γ point. Extensive discussion of nodal loops in Cu2Si monolayer can be found in a previous study by Feng et al.16 Moreover PDOS of Cu2Si monolayer reveals that the major contribution to the states around the Fermi level originates from Cu-d and Si-p orbitals. Analysis on the various ground state magnetic orders reveals that the ground state of the pristine monolayer of Cu2Si is nonmagnetic as previously reported by Yang et al.15
The investigation of adsorption of a single H atom on Cu2Si monolayer is essential for understanding the possible hydrogenation scenarios of the material. In order to simulate an isolated H adatom, the size of the supercell is chosen to be 3 × 3 × 1. While having the same electronegativity of 1.90 (in Pauling scale) provides isotropic Si–Si and Cu–Cu bonds, the difference in their electron affinities (Cu: 118.4 and Si: 133.6 kJ mol−1) causes a difference in their hydrogen adsorption process. It is expected that the Si atom provides a stronger attraction on H atom than the Cu atom. For the adsorption process of a single H atom, there are five different high-symmetry lattice sites: Si, Cu, hollow, bridge site between Cu and Si atoms (BCu–Si) and bridge site between the two Cu atoms (BCu–Cu) which are shown in Fig. 2(a). H atoms placed at the BCu–Cu and the Cu sites, settle at those sites with binding energies of −2.18 and −1.72 eV, respectively. However, when the H atom is located on the BCu–Su and the hollow sites, it moves towards Si site and settles. When a single H atom is placed directly on top of Si atom, it settles at this site with a binding energy of −2.80 eV. Therefore, Si is the most favorable lattice site for the H adatom with a calculated Si–H bond length of 1.51 Å. This value is close to the reported experimental Si–H bond length in silane (1.46 Å)42 and the calculated bond length from the summation of the covalent radii of Si and H atoms (rSi + rH = 1.42 Å). According to Bader charge analysis, Si atom transfers 0.6e charge to the H atom which gives a partial ionic character to the Si–H bond.
In order to find the migration path of H atom on Cu2Si monolayer, variation of its total energy on different lattice points is also analyzed. The energy barriers that the adsorbed H atom encounters are demonstrated in Fig. 2(a) and (b), respectively. For the calculation of the energy landscape, the position of the H adatom relative to the surface is fixed while its movement along the perpendicular direction is allowed. The paths considered are shown with black dashed lines in the inset of Fig. 2(a). The results show that the lowest energy barrier is 0.72 eV which occurs when the H atom moves from one Si site to another through the BCu–Cu. The migration path of Si–H–BCu–Cu–H–Si is presented with the green dashed arrow in Fig. 2(b). Diffusion over the Cu site has the highest energy barrier which is calculated to be 1.09 eV.
The contribution of a single H adatom to the electronic band structure of Cu2Si monolayer is also investigated. Folded electronic band dispersion of 3 × 3 × 1 monolayer of a single H atom adsorbed Cu2Si is shown in Fig. 2(c). It is seen that adsorbed H atom does not change the metallic character of Cu2Si monolayer. Moreover, the nonmagnetic ground state of the material is not affected by the adsorption of the H atom.
For the hydrogenation process, it is essential to understand the interaction between the H adatoms. We investigate 3 × 3 × 1 monolayer of Cu2Si in which two H adatoms are bonded to the Si sites from (i) one side (single-sided) and (ii) both sides (double-sided) of the monolayer. Since the separation of the two nearest Si sites is equal to 4.10 Å, the coupling between two H adatoms is negligible. The binding energies of single-sided and double-sided structures are calculated to be −2.68 and −2.66 eV, respectively. The bond strength between the Si and H atoms in the H-adsorbed Cu2Si is weaker than the one between two H atoms in the H2 molecule (−4.54 eV). Thus, for the hydrogenation of the pristine monolayer, an extra energy is required to dissociate the hydrogen atoms of the H2 molecule. In order to validate this discussion, adsorption of a H2 molecule on Cu2Si is also investigated and it is found that H2 molecule is physisorbed ∼4 Å above the pristine monolayer of Cu2Si with a weak vdW interaction of −0.20 eV. For this reason the hydrogenation of Cu2Si monolayer is only possible with the atomic hydrogen (which can be produced by hot wire chemical vapor deposition43,44). Feasibility of the hydrogenation is possible with the atomic hydrogen processes by doing plasma hydrogenation; in particular, plasma hydrogenation is used in synthesis of graphene.45
For the monolayers highH-s and highH-d, the H concentration is doubled. The monolayers of highH-s and highH-d contain 4 and 16 atoms in their unit cells, respectively. Compared to the pristine monolayer, the lattice constants for both of the structures are found to increase less than 1%. Although the monolayer of highH-s preserves its perfect hexagonal lattice structure, it is found that the monolayer of highH-d is slightly distorted. Calculated bond lengths of Si–H for the monolayers of highH-s and highH-d, are 1.51 Å and 1.52 Å, respectively. For highH-s and highH-d structures, the average electron donation of Si atom to H atom is calculated to be same with a value of 0.6e.
Fig. 3 Top and side views, and phonon band structures of the hydrogenated monolayers: (a) lowH-d, (b) highH-s, and (c) highH-d. |
Since the unit cells of the pristine Cu2Si and highH-s are similar, their phonon band diagrams can be directly compared. Although there is a resemblance between their phonon band diagrams, LO and TO modes of pristine structure soften in the hydrogenated structure. Since Si atoms donate electron to the H atoms, the in-plane bonds of Si with Cu weaken and this leads to a decrease in the mode frequencies. On the other hand, ZO modes dominated by the Cu motions harden (which is discussed in Sec. IV C).
Furthermore, it is seen from the Fig. 3(a)–(c), the soft phonon mode previously seen at the M point of the phonon band diagram of Cu2Si monolayer disappears when the material is hydrogenated. Differing from the pristine Cu2Si, hydrogenated derivatives have high-frequency modes between 2000-2100 cm−1 (see Fig. 3) indicating the formation of strong Si–H bonds. H atoms are relatively much lighter than the Si and Cu atoms and thus, it is expected that the phonon modes that correspond to the Si–H bonds have much higher frequencies. These high-frequency modes have out-of plane character and include out-of-phase motions of Si and H atoms in all cases.
The effect of the hydrogenation on the constant-volume specific heat of the material is also investigated. The specific heat of structures as a function of phonon frequency, w, is calculated as follows,46
(2) |
Atom-projected partial phonon DOS of pristine and hydrogenated derivatives of Cu2Si monolayer are presented in Fig. 4(a). At the low frequencies (i.e. < 300 cm−1), it is seen that the main contribution to the DOS comes from the Cu atoms, whereas the DOS of Si atoms dominate at relatively high frequencies (from 300 to 430 cm−1) as expected from the masses of these atoms. In the highest frequency region (i.e. > 500 cm−1) contribution of the H atoms are dominant. The contribution of the Si atom in this region to the phonon DOS reveals the interaction of Si and H atoms.
Temperature dependent variation of the derivative of the phonon occupation functions are also illustrated in Fig. 4(a). These functions determine the contribution of vibrational modes to the specific heat of a material. It is evident that the hydrogen modes, which have very high frequency values, contribute more to the specific heat of the material at high temperatures. As a result of this, as the amount of hydrogenation increases, the higher temperature specific heat of the material also increases (see Fig. 4(b)). Moreover, it is well known that the hydrogenation of a material leads to decrease in its mass density which gives rise to an increase in its specific heat at high temperatures. As the temperature is lowered, the specific heat values of all these structures get close to each other, and at temperatures around 100 K, they merge to the same value. As the temperature is further lowered (around 20 K), the specific heat of pristine Cu2Si becomes higher than those of the hydrogenated derivatives. A similar crossover in the specific heat values is also reported for graphite and diamond structures.47 At room temperature specific heat values of Cu2Si, lowH-d, highH-s and highH-d are calculated to be 438, 470, 507 and 508 J kg−1 K−1, respectively. Moreover, in the inset of Fig. 4(b) the specific heat per atom of all the structures are also presented. As seen from the figure the pristine structure approaches the Dulong–Petit limit at much lower temperatures than the hydrogenated derivatives. Debye temperature values are calculated to be 429, 867, 1102, and 1078 K, for Cu2Si, lowH-d, highH-s and highH-d, respectively.
As already mentioned in Sec. III, pristine Cu2Si is a metal and possesses nodal lines in its electronic structure. Electronic band dispersion and PDOS of hydrogenated derivatives of Cu2Si are shown in Fig. 5. For the sake of comparison, the band structure of the pristine Cu2Si is also added. As seen in the figure all of the hydrogenated derivatives preserve the metallic character as the pristine one. Although Cu2Si monolayer possesses robust metallic character against hydrogenation, some deviations appear in the electronic structure as the hydrogen concentration increases. It is clearly seen that while the two nodal lines of pristine Cu2Si reside between Γ and M points at 0.6 and 1.1 eV below the Fermi level, as the amount of hydrogen coverage increases, these nodal lines appear closer to the Fermi level (EF) and at higher energies for lowH-d and highH-d, respectively. As seen in Fig. 5 (b) and (c), an energy gap occurs between the nodal lines which reside between Γ and M points.
To better understand the effect of H atoms on the electronic structure of Cu2Si, we also analyze PDOS of the hydrogenated derivatives. As previously mentioned in Sec. III, the main contribution to the electronic structure around the Fermi level of the material originates from the Cu-d and Si-p orbitals. As seen in the Fig. 5 with increasing amount of hydrogen, the contribution from Si-pz near the Fermi level decreases, and the hybridization between the orbitals of Si-pz and Cu-d decreases. It is clearly seen from the PDOS diagrams of hydrogenated derivatives of the material peak positions and the shapes of the H-s and Si-pz are overlapped which indicate the strong hybridization of these orbitals. As a result, the Si-pz peak in PDOS of the pristine crystal dissolves and moves to lower energies when the structure is hydrogenated. Bonding states of Si–H reside about 2 eV below the EF whereas the anti-bonding states of H-s are 2 eV above the EF. The saturation of the dangling bonds of Si-pz leads reduction of the surface activity of the Cu2Si monolayer. In addition, the calculations reveal that hydrogenated derivatives of the material do not exhibit any net magnetic moment.
Adsorption of a single H atom on Cu2Si monolayer was examined and the total energy calculations revealed that the most favorable adsorption site of H atom is Si site with a binding energy of −2.80 eV. Diffusion energy barrier and possible migration paths of a single H adsorbed on the structure were determined. Structural optimizations and phonon calculations revealed that there exists three dynamically stable hydrogenated monolayers of Cu2Si. It was found that the planar geometry and the metallic electronic character of the material were not affected by different amounts of hydrogenation and the specific heat of the material at room temperature increases as the amount of hydrogenation increases. Cu2Si monolayer with a planar geometry and robust electronic structure offers a new platform for nanoscale applications.
Footnotes |
† PACS numbers: 71.15.Mb, 61.72.Ww, 63.20.Dj, 63.20.dk, 65.40.Ba, 73.22.-f. |
‡ Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra07824f |
This journal is © The Royal Society of Chemistry 2018 |