Open Access Article
Zhenbang
Zhang
ab,
Rongjie
Yang
a,
Yandong
Wang
a,
Kang
Xu
a,
Wen
Dai
a,
Jianxiang
Zhang
a,
Maohua
Li
a,
Linhong
Li
a,
Yingying
Guo
a,
Yue
Qin
a,
Boda
Zhu
a,
Yiwei
Zhou
a,
Xingye
Wang
a,
Tao
Cai
ac,
Cheng-Te
Lin
ac,
Kazuhito
Nishimura
ac,
Hao Nan
Li
*b,
Nan
Jiang
*ac and
Jinhong
Yu
*ac
aKey Laboratory of Marine Materials and Related Technologies, Zhejiang Key Laboratory of Marine Materials and Protective Technologies, Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, Ningbo 315201, China. E-mail: yujinhong@nimte.ac.cn
bNottingham Ningbo China Beacons of Excellence Research and Innovation Institute, University of Nottingham, Ningbo, China
cCenter of Materials Science and Optoelectronics Engineering, University of Chinese Academy of Sciences, Beijing 100049, China
First published on 7th August 2024
As electronic devices advance, there's a critical need for thermal interface materials (TIMs) with high thermal conductivity and minimal thermal resistance to address thermal dissipation challenges effectively. Carbon fibers (CFs), known for their axial thermal conductivity, are ideal for creating high-performance TIMs in a vertically aligned structure, aligning with the TIMs' heat transfer direction. Despite advancements in CF alignment for improved thermal conductivity, the high thermal resistance and the need for cost-effective manufacturing remain challenges. We propose a novel sandwich structure integrating vertical heat transfer pathways with surface modification to tackle these issues. This structure features a core of vertically aligned CF composite, achieved through a rolling-press method, flanked by liquid metal-modified layers to reduce contact thermal resistance. Our composites demonstrate an exceptional through-plane thermal conductivity of 51.90 W m−1 K−1 at 73.68 wt% filler content, 323 times higher than that of the PDMS matrix, and a reduced total thermal resistance from 0.55 to 0.32 K cm2 W−1 after interface modification. This research offers insights into designing CF-based composites for enhanced thermal management, applicable in cloud computing and autonomous driving.
Thermal conductivity enhancement relies not only on filler loading but also on the morphology of the fillers (including size, aspect ratio, and alignment) and the interfacial thermal resistance between fillers and the substrate.9 Previous research findings indicate that fillers with high aspect ratios surpassing the percolation threshold establish continuous heat transfer pathways, achieving efficient heat transfer. Pitch-based carbon fibers (CFs), as one of the prime candidates for high thermal conductivity fillers, exhibit ultra-high axial thermal conductivity (900 W m−1 K−1) and outstanding thermal stability.25 Their high aspect ratios and micron lengths facilitate easier alignment and interconnection, forming continuous thermal pathways to augment the thermal conductivity of composites. To maximize the thermal transport capabilities of CFs, numerous strategies have been reported to achieve their vertical alignment within polymer matrices. These strategies include ice-templating,26 electrostatic flocking,27 magnetic field assistance,28 stress-induced orientation,29 and flow-assisted methods.30 Ma et al. utilized a vertical freeze-drying method to fabricate a 3D CF skeleton, resulting in an epoxy composite with a through-plane thermal conductivity of 2.84 W m−1 K−1 at only 13 vol% filler content.31 Wu et al. applied gravity-driven ice-template methods to establish a horizontal CF heat transfer pathway, achieving an in-plane thermal conductivity of 7.98 W m−1 K−1 at a 22.3 vol% CF content in the composite.32 Due to limitations in the ice crystal growth-driving force, achieving consistent orientation at high filler content becomes challenging. Huang et al. prepared PDMS composites employing a flow-field technique to bridge Al2O3 particles with vertically aligned CFs, achieving a through-plane thermal conductivity of 38.0 W m−1 K−1 with 24 vol% CFs and 47 vol% Al2O3.33 In Han's work, they controlled the orientation of diamagnetic CFs by manipulating the direction of the magnetic field, achieving a maximum thermal conductivity of 45.01 W m−1 K−1 in the composite.34 Despite researchers employing various techniques to orient CFs and achieving outstandingly high thermal conductivity, the actual heat transfer efficiency of these as TIMs remains unsatisfactory. The mating surfaces of TIMs with vertical CF structures exhibit significantly high Rcontact when connected to the heat sink and heat source. This is primarily attributed to the raised and uneven height of the CFs on the surface of TIMs. Due to the high modulus of the CFs, they are unable to deform adequately under normal packaging conditions to establish extensive and efficient contact with the heat sink and heat source. The insufficient contact significantly undermines the effectiveness of heat transfer across the mating interface, presenting a common challenge encountered by nearly all vertically aligned CF-TIMs. To achieving genuinely efficient heat transfer requires not only advancing the κ⊥ of vertically aligned CF-TIMs through structured modulation but also optimizing the contact status between TIMs and the heater/heat sink to minimize the Rcontact.
Herein, we developed a sandwiched structure incorporating a dual strategy of vertical heat conduction pathways and interface modification. The middle layer features vertically aligned CF heat conduction pathways to enhance κ⊥, while the upper and lower layers consist of liquid metal-modified layers to reduce Rcontact. The rolling–stacking process employed in this study enables the continuous and large-scale fabrication of composites featuring a vertically oriented CF structure. Based on its rational structural design, the vertically aligned CF and BN (VCB) composite achieved a maximum κ⊥ of 51.90 W m−1 K−1, while also exhibiting outstanding thermal stability and good compressibility. Additionally, the introduced liquid metal-modified coating transformed the contact state at the interface from “elastomer–solid” to “liquid–solid” due to which the total thermal resistance of TIMs decreased to 0.32 K cm2 W−1. Moreover, the impact of the vertically aligned CF structure on the thermal conductivity of the VCB composite under compressive deformation was discussed. In real dynamic applications like CPU cooling down, the VCB composite demonstrated outstanding heat transfer capabilities. This work provides new insights into the design and fabrication of CF-based composites, leveraging their vertical structure and superior heat dissipation performance, offering potential solutions for high-power, high-frequency chips, and consumer electronics in thermal management.
:
1 ratio using a high-speed mixer (2000 rpm, 2 minutes) to achieve uniformity. Subsequently, a predetermined proportion (55, 60, 65, 70, and 73.68 wt%) of CFs and BN fillers (maintaining a fixed ratio of 8
:
1 for CFs to BN) is added to the prepared PDMS solution. Due to the high filler content, achieving uniform mixing of the solution requires multiple sequential additions of fillers during the mixing process. This step also involves the use of a high-speed mixer operating at 2000 rpm for a duration of 5 minutes to ensure thorough mixing. The second step involves orienting the CFs using a roll press machine. The uncured mixed solution is poured into the hopper of the roll press machine, with a layer of PET film placed above and below (to maintain the shape of the uncured material). The distance between the dual rollers is adjusted to control the degree of fiber orientation, with the rollers operating at a controlled speed of 60 cm min−1. Subsequently, the oriented thin-layered CF composite is cured for 12 hours at 80 °C. The third step involves preparing block-shaped composites. Post-curing, the high-viscosity thin-layered composite necessitates the removal of PET film with the assistance of liquid nitrogen. A stacking-friendly shape is achieved by using a template cutter along the fiber orientation direction. Finally, the stacked composite is placed in a specialized mold and subjected to a pressure of 20 MPa to densify the composites. Subsequently, the block-shaped composite material is sliced along a specific direction using an ultrasonic cutter.
The strategy of this study involves filling polymers with fillers and modifying their arrangement to enhance the thermal conductivity of composites. Consequently, the properties and dimensions of the fillers will directly impact the overall performance of the composites. In our study, high thermal conductivity short chopped pitch-based CFs were chosen as the primary filler to enhance the thermal conductive of the composite. Fig. S7a–c† depict the optical, SEM magnified, and microstructural images of CFs. According to the images, the diameter of the CFs measures 10 μm, with a length of 250 μm (as detailed in the length distribution in Fig. S7d†). Furthermore, the fiber cross-section displays the characteristic radial folded arrangement indicative of mesophase pitch-based CFs. The XRD pattern of the CFs displayed in Fig. S7e† exhibits characteristic peaks associated with graphite, and the peak at 26.4° corresponds to the (002) plane, while the prominent peak at 54.5° is assigned to the (004) plane. These sharp characteristic peaks indicate larger grain sizes, smaller interlayer spacing, and a closely packed arrangement of graphite layers, consistent with the cross-sectional image in Fig. S7c.†37 The Raman spectrum of the CFs is depicted in Fig. S7f,† wherein distinct peaks at 1353, 1582, and 2704 cm−1 labeled as D, G, and 2D, respectively, were observed. These peaks are commonly employed to characterize the structure of carbon materials, and the ID/IG ratio of the CFs serves as a pivotal metric for assessing their thermal conductivity. The ID/IG value of the CFs utilized in this study is 0.135, indicating remarkably low defects and superior thermal conductivity. h-BN serves as the second hybrid filler in this study. Its role includes filling the gaps between CFs, bridging these fibers to establish additional thermal pathways. Furthermore, it aids in modulating the rheological properties of the uncured mixed solution. The optical and SEM magnified images of the h-BN are presented in Fig. S8a–c.† The h-BN exhibits a lateral size range of 20–50 μm, as depicted in the lateral size distribution plot in Fig. S8d,† with a thickness of 1–2 μm. Fig. S8e† displays the XRD pattern of BN, showcasing distinct characteristic peaks. Additionally, Fig. S8f† presents the prominent Raman peak at 1365 cm−1 for h-BN. These results confirm the excellent crystal quality of the larger-sized BN.
Based on their fabrication method, the produced block-shaped composites exhibit anisotropic characteristics. To explore their internal structure and the influence of fiber orientation on performance, samples were sliced along the direction indicated in the schematic diagram in Fig. 2a. The composites cut along the direction perpendicular to the Cartesian coordinate system's X-axis are denoted as VCB-X, featuring a vertical CF alignment within their interior. Correspondingly, samples cut along the direction perpendicular to the Y and Z axes are denoted as VCB-Y and VCB-Z, respectively. To analyze the internal structure, we used an advanced micro-CT tool to scan the VCB-X, VCB-Y and VCB-Z composites. Within this research, the angle between the fibers and the Z-axis (through-plane direction) was defined as θ, as illustrated in Fig. 2b. Furthermore, the CF skeleton inside the three composites is shown in Fig. 2c (where fibers at different angles are represented by distinct colors). ESI Video S1† showcases the angular distribution of CFs in the three specimens. Subsequently, reconstruction of models was conducted using analysis software, generating the fiber angle distribution data within each composite, as depicted in Fig. 2d. By comparing the data from the three specimens, the angular distribution of the VCB-73.68 wt%-X specimen follows a normal distribution centered at 15°. Correspondingly, the model predominantly exhibits blue and green colour, which aligns with our deliberately controlled outcome (smaller angular distributions indicate higher alignment degrees). However, in VCB-73.68 wt%-Y, the distribution appears more random, leading to a relatively chaotic pattern in the model. However, the VCB-73.68 wt%-Z sample exhibits a predominance of larger angular distributions, resulting in a higher uniformity in the model colors. Yet, due to the low radial thermal conductivity of CFs, this orientation in this direction does not favor through-plane heat conduction. Considering the significantly higher axial thermal conductivity of the anisotropic CFs compared to their radial counterpart, we introduced the parameter of “effective fraction”. When θ is less than 45°, it signifies a higher contribution to heat conduction; however, angles greater than 45° contribute less. Through calculations, the VCB-73.68 wt%-X sample exhibited an effective fraction of 59.14%, VCB-73.68 wt%-Y measured 36.87%, while VCB-73.68 wt%-Z was only 1.66%. Wide-angle X-ray diffraction (WAXD) was utilized to assess the degree of orientation in composites. CFs comprise stacked layers of hexagonal carbon networks preferentially oriented along the fiber axis, with the structural and orientational characteristics revealed by the XRD peak originating from the (002) crystal plane reflection of these carbon network layers.38,39 Employing this technique, an analysis was conducted on three variants of VCB composites, and the resultant 3D and 2D patterns are visually presented in Fig. 2e. During the test, X-rays directly pass through the actual heat transfer path of each sample. Due to the vertical distribution of CFs in the VCB-X sample, X-rays passing through the axial direction of the fibers do not exhibit noticeable characteristic peaks. However, in the VCB-Y and VCB-Z samples, X-rays passing through the radial direction of the fibers exhibit distinct peaks that are clustered together. The diffraction peaks of VCB-Z have a relatively narrow half-width, consistent with the micro-CT test data. Fig. S9† also displays the integral intensity of the (002) crystal vs. azimuth angle curves of the three samples. Through the aforementioned testing methodologies, we have successfully fabricated anisotropic composites with highly oriented structures. Among these, VCB-X exhibits the most promising vertical alignment of CFs. This vertical structure establishes the most efficient thermal conduction pathway, greatly enhancing the thermal conductivity efficiency of the thermal interface material.
![]() | (1) |
338%, as shown in Fig. 3e, whereas the VCB-73.68 wt%-Z at the same filler content registers only 1194%. This data further validates the crucial significance of controlling the orientation structure of anisotropic fillers.
Beyond thermal conductivity, thermal stability also dictates the applicability of certain materials. Excellent thermal stability allows materials to perform effectively under extreme operating conditions. Fig. 3f illustrates the thermal conductivity change of VCB-73.68 wt%-X across a temperature range of 25 to 115 °C. As expected for many materials, there is a gradual reduction in thermal conductivity with increasing temperature. Fig. 3g records the variations in thermal conductivity during successive heating and cooling cycles, aiming to assess the stability of thermal conductivity under thermal shock conditions. The graph displays ten cycles of heating and cooling. Throughout this phase, VCB-73.68 wt% demonstrates commendable stability, displaying minor fluctuations, both at high and low temperatures. In Fig. 3h, we have compared the thermal conductivity values of previously reported CF-based TIMs with those obtained in this work, considering the preparation techniques employed for oriented CFs. More detailed data can be found in ESI Table S2.† Methods like ice templating26,31,40 are suitable for fabricating 3D skeletons, yet they fail to provide high thermal conductivity at low filler concentrations. Techniques such as electrostatic flocking27,41,42 and magnetically assisted methods,28,34,43 due to their intricate process conditions, have not gained industrial acceptance. Presently, methods involving 3D printing23,30,33 and flow-assisted extrusion,44 as well as the pre-arrays45–47 of continuous CFs, appear to hold promise as potential industrial-scale manufacturing processes for TIMs. It is worth noting that both 3D printing and flow-assisted extrusion techniques seem to have reached a bottleneck in terms of achieving thermal conductivity improvements, as neither has surpassed 40 W m−1 K−1. Moreover, while the approach involving continuous pre-alignment of CFs holds promise for achieving higher values, the cost of continuous CFs remains prohibitively high for manufacturers. Therefore, the rolling-press technique48 employed in this study emerges as a potential method for large-scale production of high thermal conductivity CF-TIMs. The TIMs produced through this method achieved thermal conductivity exceeding 50 W m−1 K−1, surpassing all previously mentioned fabrication approaches. The density of TIMs is also a crucial parameter under consideration. In Fig. 3i, a comparison of density vs. thermal conductivity is drawn among CF-based TIMs,29,30,34,45 BN-based TIMs,49–53 and commercially available CF-based TIMs from previous literature. The detailed parameters are provided in Table S3.† It's observed that most TIMs exhibit a density below 2 g cm−3, owing to the relatively lower density of CFs and boron nitride fillers. However, the thermal conductivity of BN-based TIMs remains below 15 W m−1 K−1, unable to meet the requirements for high thermal conductivity. While commercially available CF-TIMs exhibit commendable thermal conductivity, they tend to have higher densities. Contrastingly, the TIMs developed in this study achieve the highest thermal conductivity alongside relatively lower densities. Therefore, this sample demonstrates significant advantages in applications requiring extreme lightweight characteristics, such as aerospace or portable electronic devices.
Furthermore, the rough surface of CF-based TIMs cannot achieve extensive interfacial contact, resulting in an increase in interfacial thermal resistance. Therefore, a low compression modulus allows the TIMs to deform under pressure, enabling them to conform to rough surfaces. Fig. S10† illustrates the compression stress–strain curve of VCB-73.68 wt%-X. The curve indicates significant deformation occurring at relatively low pressures, implying that this TIM can achieve excellent conformability even at lower packaging pressures. Another point of interest is that the vertically structured TIMs, upon experiencing deformation under pressure, cause a tilt in the angles of the CFs, as depicted in the schematic diagram of Fig. 4a and S11.† While we aim to prevent tilting, the alteration in the anisotropic structure under substantial deformation is unavoidable. Hence, determining the optimal sealing pressure for anisotropic TIMs is an essential consideration. Fig. 4b illustrates the change in thermal conductivity and thickness of VCB-73.68 wt%-X upon deformation under pressures ranging from 10 to 100 psi. It's important to note that the thickness measurements were taken after compression. As depicted in Fig. 4b, with increasing pressure, the thickness of VCB-73.68 wt%-X decreased from its original 1.40 to 0.80 mm after compression at 100 psi, concurrently reducing the thermal conductivity from 50.62 to 19.07 W m−1 K−1. As evident in Fig. 4c–e, prior to compression, the CFs in the TIMs were positioned at a 90° angle to the base. Following compression at 50 psi, the CF angle changed to 51°, further reducing to 38° after compression at 100 psi. Based on the above results, we determined that the optimal packing pressure range for VCB composites is 10–30 psi. Within this range, the inclination angle of the CFs does not change significantly. However, when the pressure exceeds 50 psi, the CFs exhibit excessive inclination, leading to a substantial decrease in thermal conductivity, thus resulting in failure.
To further validate the impact of CF orientation angles on thermal conductivity, finite element analysis was employed for verification. The first step involved establishing four models as depicted in the Fig. S12,† positioned at the same heating plate, while the external surroundings were designated as PDMS substrate with a thermal conductivity of 0.16 W m−1 K−1. Within the substrate, CFs were introduced at angles of 0°, 30°, 60°, and 90° respective to the base. The ambient temperature was set at 22 °C, and convective heat transfer conditions were applied to the boundaries of the four models, with a coefficient of 5 W m−2 K−1. The heating plate was maintained at a constant 80 °C, ensuring heat conduction from the bottom of the model to the top. The boundary conditions were set for the models, and subsequently, a mesh generation process was applied to the configured models, as depicted in Fig. S13.† Following this, computations were performed, producing temperature distribution maps for the four models, showcased in detail in Fig. 4f. As indicated by the computational outcomes, the inclined angle of CFs significantly influences the temperature distribution within the models. Fig. 4g illustrates the temperature gradient from the bottom to the top within the models. The model with a 0° orientation of CFs exhibits the most significant temperature differential, reaching only 58.2 °C at the top surface. Conversely, the model with a 90° orientation shows the best internal temperature uniformity, reaching 73.9 °C at the top surface. Additionally, the model tilted at 60° demonstrates better temperature uniformity compared to the 30° oriented model. This simulation outcome aligns with our experimental results, indicating that an increase in the tilt angle of CFs leads to a decrease in their thermal conductivity.
![]() | (2) |
In Fig. 5b, the optical images reveal distinct appearances between the original VCB-73.68 wt%-X and the liquid metal modified VCB-73.68 wt%-X-LM. The original TIM presents a dark, CF-like hue, while the VCB-73.68 wt%-X-LM showcases a metallic luster resembling liquid metal. In Fig. 5c, the SEM images display the cross-sectional view of VCB-73.68 wt%-X-LM, while Fig. 5d–i illustrate the corresponding elemental distribution maps. These findings provide evidence that the liquid metal has been uniformly applied to the sample surface, with a thickness ranging approximately between 10 and 15 μm. Fig. 5j displays the microscopic morphology of VCB-73.68 wt%-X-LM, while Fig. 5k and l illustrate a comparative analysis of the surface structures between VCB-73.68 wt%-X and VCB-73.68 wt%-X-LM. It's evident that the surface of the original sample is filled with upright CFs and exhibits some pores. The surface roughness (Sa) of the original sample was measured to be 15.29 μm through laser confocal testing, with detailed results illustrated in Fig. S14a–c.† The high surface roughness is a crucial factor affecting Rcontact. Due to the notably high modulus of CFs and the significantly lower modulus of the PDMS matrix, there is currently no effective method available to achieve a uniformly smooth surface for this composite through mechanical slicing. Surface modification has become an effective way to achieve low roughness for this composite. Through observation, the surface of VCB-73.68 wt%-X-LM is entirely covered by the liquid metal, effectively filling the surface pores. The surface roughness (Sa) measures 14.32 μm as shown in Fig. S14d and e.† The limited reduction in surface roughness is attributed to the high surface tension of the liquid metal, causing small droplets to re-aggregate, forming larger droplets. These droplets create surface protrusions, which result in the higher surface roughness. However, this high roughness is deceptive and the protrusions tend to flow, enhancing the conformability of the interface.
As depicted in the schematic diagram in Fig. 5m, under normal packaging pressure, the low-modulus TIMs can undergo some deformation to conform to the rough surfaces of both the heat sink and heater, thereby increasing the effective contact area. However, there still exist tiny voids in micron size that cause thermal resistance. Due to its excellent flowability, liquid metal can almost perfectly fill the voids between interfaces, forming a “solid–liquid–elastomer” structure, significantly increasing the effective contact area and thereby enhancing heat transfer efficiency. Next, we tested the total thermal resistance of VCB-73.68 wt%-X and VCB-73.68 wt%-X-LM using the ASTM D-5470 standard, and the results are depicted in Fig. 5n. The total thermal resistance of untreated VCB-73.68 wt% ranges from 0.75 to 0.48 K cm2 W−1 under 10–100 psi pressure, decreasing with increasing pressure. However, for VCB-73.68 wt%-X-LM samples, the thermal resistance is only 0.44–0.26 K cm2 W−1. Compared to before modification, there's a significant decrease in total thermal resistance, attributed to the effectiveness of the liquid metal buffer layer. Fig. 5o illustrates a comparison plot presenting the thermal conductivity and total thermal resistances of various types of TIMs reported in previous literature, such as hydrogels,54,55 thermal pads,47,56–59 and thermal grease.60,61 The detailed parameters are outlined in Table S4 of the ESI.† Despite the notably low thermal resistance in certain thermal greases, their thermal conductivity tends to be low, and these low resistances are often measured under extremely thin BLT. In applications demanding thicker BLT, thermal pads demonstrate their advantage. In comparison to other pads, our VCB-73.68 wt%-X-LM in this study achieves the highest thermal conductivity and remarkably low thermal resistance. This is evident upon contrast with other existing thermal pads.
Considering the exceptional heat transfer capabilities of the produced VCB-73.68 wt%-X-LM, we directly integrated it into a commercial desktop computer to validate its thermal behavior in real dynamic applications. As illustrated in Fig. 6e and depicted in the optical photograph, VCB-73.68 wt%-X-LM was packaged as a TIM between the Central Processing Unit (CPU, Inter core i5) and the air-cooled heat sink. Then, professional system diagnostic software (OCCT) was employed to drive the CPU to run at 100% usage. Meanwhile, the software HWINFO64 was utilized to monitor the temperature evolution of the CPU core and the effective clock frequency. For comparison, we conducted CPU stress tests under the same conditions using VCB-73.68 wt%-X and without using TIMs. As shown in Fig. 6f, under normal state, employing VCB-73.68 wt%-X-LM as the TIM decreased the temperature of the CPU core (TCPU core) by 4 °C compared to that without using the TIM, and it decreased by 2 °C compared to using VCB-73.68 wt%-X as the TIM. During the stress test stage, the temperature gap increased notably. The TCPU core with VCB-73.68 wt%-X-LM as the TIM dropped by 8 °C compared to when no TIM was used. It also showed a 2 °C decrease compared to using VCB-73.68 wt%-X as the TIM. Here we noticed a discrepancy between the CPU test results and the TIM performance test results. It's important to note that during the CPU stress test, we utilized the existing commercial heat sink and fan, which have limited convective heat dissipation capabilities. While VCB-73.68 wt%-X-LM efficiently conducts CPU heat to the heat sink, the fan isn't able to promptly remove the heat from the heat sink, hindering the CPU temperature decrease. Despite the impact of the heat sink and fan on the TIM performance, as depicted in Fig. 6g, employing VCB-73.68 wt%-X-LM as the TIM resulted in an increased effective CPU clock frequency of 52.6 MHz compared to operating without a TIM. The increase in the effective CPU clock frequency directly enhances user experience, validating the potential application of VCB-73.68 wt%-X-LM as the TIM in the realm of consumer electronics.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ta03924f |