Samuel R.
Wilson-Whitford
*ab,
Maria Chiara
Roffin
ac,
Jinghui
Gao
a,
Thitiporn
Kaewpetch
d and
James F.
Gilchrist
*a
aDepartment of Chemical and Biomolecular Engineering, Lehigh University, Bethlehem, PA, USA. E-mail: gilchrist@lehigh.edu
bSchool of Chemistry, University of Leicester, Leicester, UK. E-mail: srww1@leicester.ac.uk
cSchool of Science and Technology, Nottingham Trent University, Nottingham, UK
dDepartment of Packaging and Materials Technology, Faculty of Agro-industry, Kasetsart University, Bangkok, Thailand
First published on 12th October 2023
Try and encapsulate microparticles inside the cores of microcapsules and you will often find that particles adhere to the liquid–liquid interface in a phenomenon known as Pickering stabilization. Particles will remain irreversibly trapped and embedded within the subsequently formed microcapsule membrane. In cases where the encapsulant particles must remain suspended inside the microcapsule core to retain their desired properties or behaviours, Pickering stabilization is detrimental. Here we demonstrate a general procedure using yield stress materials as the core material, where the yield stress of the gel is strong enough to suspend particles against sedimentation, but weak enough to allow spatial manipulation of encapsulant particles using an external field. This external field imparts enough force on particles to disrupt the supporting network and allow particle mobility after encapsulation.
If we emulsify two immiscible phases in the presence of small particles (in either the dispersed or continuous phase), we can in many cases expect the resultant droplets to be stabilised by the particles as they adsorb to the interface in a phenomenon known as a Pickering stablisation.8–10 This is due to the substantial energetic advantage of particle adsorption to a fluid–fluid interface.11,12 The microparticles in this case arrive at the interface as a result of Brownian diffusion or sedimentation. This processes can, in some cases, be a desirable phenomenon and in fact has given rise to the study of armoured droplets known as “colloidosomes”.13,14 In other cases, it can be desirable to produce microcapsules which contain a suspension of particles throughout the core. It has been shown that when generating droplets from an organic phase laden with particles, the particles will almost instantaneously saturate the interface.15 For this reason it is important to develop synthetic approaches that control the behaviour of encapsulated suspensions of microparticles during the encapsulation process.
One approach to create microencapsulated suspensions is to avoid the presence microparticles during the membrane/shell formation and to nucleate particles in situ after encapsulation is complete. This has been shown through emulsion polymerization techniques,16–18 template-free methods and Ostwald ripening methods,19 but these approaches often produce materials where the chemistry of the core and shell are the same. Alternatively, low Reynolds number approaches such as microfluidics are employed.20,21 Microfluidics has the added advantage of being able to use external fields to influence microparticle diffusion and motion inside droplets.22–25 Other approaches have utilised layer-by-layer templating syntheses. Here microparticles can be coated within a sacrificial layer which is chemically etched after an outer shell has been formed to give “yolk–shell” or “microrattle” morphologies.7,26–28
The most practical approaches available in the literature are based on the arrest of particle Brownian diffusion or sedimentation through control of the dispersed phase's rheological properties by methods such as core gelation/solidification,29–34 or through solvent-particle density matching.35,36 Perhaps a forgotten technique in this category is reliquification, where microcapsules are formed with a solid gel core, usually an ionic crosslinked alginate gel, and the cores are subsequently reliquefied by addition of a chelating agent, such as EDTA.37–39 This has proven to be an effective technique for encapsulation of living tissues/particulates. This approach is easily applicable to aqueous core capsules, due to the large variety of available hydrogelators, but this technique has limited scope for oil-in-water (O/W) systems due to lack of suitable materials. With this in mind, a similar concept using oil-soluble yield stress materials, such as hydrogen bonded gels could be used as an analogous O/W method.
The synthetic route proposed herein is the use of an oil-based core material that possesses a yield stress strong enough to counteract the effects of gravity and Brownian motion but weak enough to yield in the presence of an external field or force (Fig. 1). Reliquification is achieved by utilizing shear rather than chemically induced triggers. In a generalised approach, we show an O/W polyurea microcapsule batch synthesis using an ethyl cellulose-dioctyl phthalate (ECDOP) dispersed phase. Micron-scale magnetic (field responsive) particles are distributed between the core and the interface of the microcapsules, depending on the particle position upon droplet generation, leaving the particles which remain in the core of the microcapsules free to be spatially manipulated by an external field. We believe this is a convenient route to larger scale synthesis of microcapsule sensors, micromixers, microreactors and field-responsive display inks, and should be treated as a generalised synthetic procedure applicable to a wide range of particle sizes, chemistries, and shapes etc.
In pursuit of the proposed mechanism shown in Fig. 1 it is important to identify a balance between particles sedimenting in the gel core and the ability to yield the network with an external force. Due to the relatively large density difference between the solvent and the particles (∼0.8–1 g cm−3) it is assumed that sedimentation due to gravity is more significant than the ability of particles to migrate to the interface through Brownian motion. To identify a transition point where particles no longer sediment, EC:DOP solutions were prepared at 0–6 wt% at 1% intervals and loaded with dispersed fluorescent particles (0.3 vol%). The experimental setup is described in S1. Samples were imaged on a confocal piezo stage over a set volume (μmx, μmy, μmz: 40, 40, 100), upward from the glass substrate (z = 0 μm → z = 100 μm). Scans were performed 15 min after sample preparation to allow for sample relaxation and again after 4 h, to mimic reaction conditions. Fig. 2 shows analysis of the sedimentation of particles in the gels at different gel concentrations. Fig. 2(a)–(f) show typical examples of the distribution of particles in the bottom 100 μm of samples, after 4 h. The particle number density reduces notably between 1–3 wt% gel and remains approximately the same between 4–6 wt% demonstrating retardation of sedimentation. Fig. 2(g) shows the average total particle count by fixed volume for each gel concentration after 15 min and after 4 h. After 15 min, the particle count is essentially equal between all gel concentrations with a slight bias to the lower concentration, but after 4 h, it is clear that a considerable amount of sedimentation has occurred in the lower concentration gels. The transition point could be indicated as lying approximately between 3–4 wt% EC.
Here, the key concern is the settling velocities of particles, and at which gel concentration would a majority of the encapsulated particles remain away from the interface during the critical first hour of the synthesis. This first hour accounts for a majority of polymer membrane formation. The ECDOP itself, from a simplistic perspective, could be considered as a viscous material in which the settling rate of particles depends on the viscosity as a function of the wt% of gel. It should be noted that for systems with much higher particle volume fractions, the percolation lengths could significantly influence gel structure and behaviour. Alternatively, in an elastic state, we could consider particle sedimentation as a probability that a particle is held by the gel network, with that probability being some function of the wt% gel, though perhaps more realistically the system should be considered a combination of these two regimes. For simplicity, we are considering the system as increasingly viscous with respect to increasing gel concentration. From the confocal data, the settling velocities, νest, of the particles in each gel are estimated and are found to closely follow the theoretical terminal velocity of a 1 μm particle in pure DOP (S2). It was found that νest = 13.8 and 9.6 μm h−1 for 3 and 4 wt% respectively. Considering the average capsule diameter as 100–150 μm, sedimentation is unlikely to result in transport of a significant number of particles to the polymerising interface during the timescale of a reaction for a 3 wt% ECDOP gel. This is in agreement with the conclusions from the settling data in Fig. 2. For an order of magnitude estimate on the yield stress when Janus particles are arrested from sedimentation, σy ≈ Δρgd ≈ 0.01 Pa, where Δρ is the density difference, g is gravitational acceleration, and d is Janus particle diameter.
In a supporting experiment, samples of EC:DOP from 1–6 wt% were prepared with 0.0066 g mL−1 of fluorescent ferromagnetic Janus particles. The advantage of using Janus particles here is that it simplifies visualization of the spatial and angular perturbations of the particles. The sample preparation was identical to the settling experiment shown in Fig. 2, using cylindrical sample holders (S1). Samples were examined by CLSM whilst under magnetic agitation and the resulting videos were analysed to extract the mean square deviation (MSD) data from particle and particle cluster trajectories within the bulk yield stress gels. It should be noted that particle clusters are present primarily due to self-assembly of ferromagnetic Janus particles, a behaviour reported in the literature.43Fig. 3 shows the results of MSD calculations, with the black line showing the average MSD over all trajectories for each gel concentration. It should be noted here that MSD calculations from multiple particle tracking experiments are designed to work for particle systems with ideal Brownian trajectories. Here particles and particle clusters have rotational components to their motion which are not accounted for in microrheology.
Typically, the displacement with time (MSD vs. τ) will have a slope, α, of >1 for a super diffusive particle, equal to 1 for a Brownian particle and 0 for stationary particle. In our case, the traditional interpretation is not valid as the particles are not passive but are instead being externally manipulated. It is also important to note that the particle motion being measured is also partially rotational, especially for dimers/clusters. However, α remains indicative of the nature of the microenvironment that the particles are experiencing. Decreasing values of α here indicate an increase in the opposing force on the translational and rotational motion of the particles by the increased gel concentration. The values of α for each sample were, 1.32, 1.05, 0.75, 0.49, 0.33, 0.19 from 1–6 wt% EC respectively. For low wt% EC, the particle motion is relatively unrestricted, as seen in Supplementary Video V1 (ESI†). From >2 wt%, particle motion is significantly restricted, a trend that is exacerbated at ≥3 wt%, and essentially stationary at 6 wt% (Supplementary Video V2, ESI†). This is in agreement with the sedimentation data from Fig. 2. What is perhaps more endearing is the shape of the MSD curves. Pronounced oscillations appear as the gel concentration increases. From concentrations ≥4 wt%, stronger, regular oscillations are observed, indicating an increasing domination of elastic domains within the fluid. The onset of these pronounced oscillations is in agreement with the observations from the settling experiments, indicating that the yielding behaviour of the EC:DOP at approximately 3 wt% is an ideal concentration for the proposed system and particle selection.
Given these observations, microcapsules were synthesised adhering to the method outlined in the Experimental section and illustrated in Fig. 4. ECDOP containing responsive particles and isophorone diisocyanate (IDI) was emulsified in PVA solution and a diethylene triamine (DETA) crosslinker was subsequently added. The method utilized interfacial polymerisation of oil-soluble IDI and water-soluble DETA crosslinker to form a polyurea capsule wall. Isocyanate-amine chemistry was chosen due to the fast rates of reaction and subsequent fast initial membrane formation.44 Capsules were synthesized using the previously identified transition concentration of 3 wt% with the results shown in Fig. 5 and Supplementary Videos V3 and V4 (ESI†). Additionally, capsules were synthesised at 0 wt% and 6 wt% to demonstrate the trapping of microparticles at the interface and within an elastic core (S3 and S4).
As seen from Fig. 5 and the supporting video, the microcapsules contain particles and particle clusters. The capsule size for the sample is measured at d[3,2] = 184.5 ± 105.3 μm and shows a broad size distribution due to the emulsification method (impeller stirrer) (S5). Upon agitation with an external magnetic field, the particles and particle clusters within the capsules are seen to move freely as they yield the gel network. Some particles are also immobile, specifically those embedded in the capsule walls. This is as a result of the emulsification process. As the particle laden gel is emulsified, some particles will inevitably be at the interface as the droplets are formed, due to the random spatial distribution of particles. Importantly, a majority of particles can be observed as mobile and in the cores of the capsules. A tracking analysis of the particles and particle clusters reveals the same smooth MSD curves which are indicative of a viscous environment. This shows that the particles are successfully yielding the gel network and moving freely after encapsulation.
Although the above synthetic method is intended to be used as a general synthetic approach, applicable to all manner of particle sizes, shapes and chemistries etc. in the following we demonstrate the utility of the method through incorporation in a visually tangible application, as an alternative to E-ink displays.36 In previous work by Gao et al.,45 it was shown that chains of ferromagnetic Janus particles can be rotated in a magnetic field giving rise to an optical dynamic range based on variable transmission of light. Others have shown similar, irreversible control of transmission through magnetic particles.46 These particles can be microencapsulated using our method to produce optically dynamic microcapsules.
This dynamic optical behaviour can be observed in Supplementary Video V4 (ESI†), where capsules containing Janus particles suspended in 3 wt% EC:DOP are shown to flash under the influence of a rotating magnetic field. V4 is a zoomed-out view of a number of capsules and so the intensity change observed is not correlated to any individual movement of particles but is an average of the collective motion. In V4 a significant majority of encapsulated particles can be seen in motion, as indicated by the macroscopic variable optical transmission. Measuring of the relative intensity difference of the capsules in a rotating magnetic field shows a transition between high and low optical transmission based on the orientation of the magnetic field, with the measured change being ∼9–10% (Fig. 6). The broad error here is due to the size dispersity of the capsules themselves, essentially giving different relative thicknesses to each capsule and thus changing the measured intensity. The advantage here with comparison to traditional E-inks, is the order of magnitude increase in refresh rate. Where E-inks rely on the translational motion of microparticles,36 here particles can simply be rotated, which occurs on a significantly faster timescale. A similar phenomenon involving the reflective properties of much larger Janus particles has also been previously demonstrate in optical devices,47–49 but never before through microencapsulation. Additionally, this technology would remove the need for expensive and brittle ITO screens and top-plates on various types of devices.
Fig. 6 Relative intensity difference of capsules in a rotating magnetic field taken by greyscale image analysis of wet capsules on glass substrate similar to that of Gao et al.44 Black line indicates averaged data, grey shows error. |
Footnote |
† Electronic supplementary information (ESI) available: Details of equipment and materials, descriptions and videos of particle agitations in bulk (V1–V2) and in capsules (V3 and V4), illustration of experimental set-up (S1), apparent settling velocities (S2), particles trapped at the membrane for 0 wt% (S3), example cluster tracking for 6 wt% sample (S4), capsule size distributions (S5), confocal images of the bottom of samples after 15 min (S6) and supplementary references. See DOI: https://doi.org/10.1039/d3sm00642e |
This journal is © The Royal Society of Chemistry 2023 |