Malinalli
Ramírez-Martínez‡
ab,
Sandra L.
Aristizábal‡
ab,
Gyorgy
Szekely
abc and
Suzana P.
Nunes
*abd
aEnvironmental Science and Engineering Program, Biological and Environmental Science and Engineering Division (BESE), King Abdullah University of Science and Technology (KAUST), 23955-6900 Thuwal, Saudi Arabia. E-mail: suzana.nunes@kaust.edu.sa; Tel: +966128082771
bAdvanced Membranes and Porous Materials (AMPM) Center, King Abdullah University of Science and Technology (KAUST), 23955-6900 Thuwal, Saudi Arabia
cChemical Science Program, King Abdullah University of Science and Technology (KAUST), 23955-6900 Thuwal, Saudi Arabia
dChemistry Program, King Abdullah University of Science and Technology (KAUST), 23955-6900 Thuwal, Saudi Arabia
First published on 30th November 2022
Membrane technology is a low-footprint and highly efficient industrial separation process. While more stable membranes could substantially contribute to modernizing the chemical industry, sustainability must be seen holistically. Polymer sources, solvents, and recycling strategies that adhere to the strategic concepts of the circular economy should be considered at the membrane design stage. Recycling plastic waste into separation membranes can help remediate the environmental impact of the current plastic pollution. Polyolefins are the most manufactured and used polymer family, and their high chemical resistance and low price are attractive for membrane preparation. However, their limited solubility in mainly non-renewable solvents at high temperatures restricts their processability and recycling. In this work, we present the use of polypropylene (PP) and low-density polyethylene (LDPE) as the source of membrane preparation by their dissolution in two bio-based and renewable solvents (α-pinene and D-limonene). The thermal properties and phase separation behavior were studied and phase diagrams were obtained. Liquid–liquid phase separation and spherulitic morphology were observed for the three studied systems. PP membranes were obtained by a thermally induced phase separation (TIPS) process employing α-pinene as a solvent, and food packaging plastic waste or commercially available PP pellets in the polymer dope solution. The obtained membranes were tested for water-in-oil emulsion separations. The influence of the polymer content and the quenching media on the morphology, mechanical and thermal properties, and water contact angle was investigated. PP membranes were fabricated with 20–30 wt% polymer contents using water at 4 °C and 20 °C as quenching media. The contact angles were higher than 150° under oil enabled efficient water-in-toluene emulsion separation, where approx. 95% water rejection and an average of 99.97% toluene purity were achieved.
Polymeric membranes lead the market over ceramic ones due to their low cost, processability, scalability, and versatility.4 They are mainly prepared by phase separation processes triggered by changes in the thermodynamic conditions. A homogeneous polymer casting solution separates into a polymer-lean phase (incipient pores) and a polymer-rich phase, following a spinodal decomposition or a nucleation and growth mechanism. The polymer-rich phase gels and solidifies, kinetically trapping the porous structure.10,11 Three of the most applied techniques are thermally induced phase separation (TIPS), non-solvent induced phase separation (NIPS), and vapor induced phase separation (VIPS), in which the phase separation is triggered by a change in temperature, solvent and non-solvent exchange in the liquid state, and exposure to a non-solvent in the gas state, respectively.12,13 To date, the membrane fabrication industry uses mainly non-renewable and toxic solvents, such as N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), and N,N-dimethylformamide (DMF), and fossil-based polymers.14–16 Such solvents and polymers have been estimated to contribute to global warming, human health threats, and fossil resource scarcity.8 In response, strategies following the principles of circular economy and green chemistry are being increasingly studied over the last few years for their implementation in membrane fabrication processes. Two examples are the utilization of greener solvents and alternative polymer sources.6,7,16–19
Greener solvents in membrane preparation such as methyl lactate, ethyl lactate, Cyrene™, PolarClean®, natural organic carbonates, ionic liquids, vegetable oil, and others, have shown good compatibility with different polymers.15,20–27 For example, Rasool et al.21 fabricated asymmetric cellulose acetate (CA) nanofiltration membranes via NIPS using bio-derived methyl lactate and 2-methyl tetrahydrofuran as a solvent and co-solvent, respectively. The optimized membranes showed a Rose Bengal (1018 g mol−1) rejection above 99% in water, making them promising candidates for applications in the nanofiltration range. Wang et al.15 used the synthetic non-toxic PolarClean® for CA dissolution to fabricate nanofiltration membranes and to dissolve polysulfone (PSF) and polyethersulfone (PES) for preparing ultrafiltration membranes via the NIPS process. Marino et al.20 reported the use of Cyrene™, a bio-solvent derived from nonfood cellulosic sources, for PES and poly(vinylidene fluoride) (PVDF) membrane preparation by NIPS obtaining pore sizes around 500 nm and pure water permeance around 550 L m−2 h−1 bar−1. Ismail et al.28 reported the fabrication of PVDF membranes employing ethylene carbonate (EC) as a solvent during a combined NIPS and TIPS process, which exhibited an outstanding performance for water desalination by membrane distillation, with more than 99.97% salt rejection factor. These encouraging works serve as an example of the high potential of green solvents for replacing traditional non-renewable ones while maintaining a competitive performance to be applied in diverse applications. Nevertheless, the use of green solvents for the dissolution of chemically stable polymers is still challenging. This is the case for polyolefins such as polyethylene (PE) and polypropylene (PP), commonly dissolved in fossil-derived hydrocarbons (e.g. p-xylene, dodecane, decalin, and paraffin oils) at temperatures ranging from 140 to 250 °C. Beside their processing limitations, PP and PE significantly contribute to plastic pollution, considering that they account for nearly half of the plastics produced worldwide for their use in applications such as food packaging, bottle containers, automotive parts, toys, and houseware products (182 million metric tons produced in 2021)29,30 and that only around 8.8% of the plastics are recycled.31,32 A 2017 report by the Ellen Macarthur Foundation estimated that plastic packaging materials are devalued by 95% after one short use, which translates to economic losses of USD 80–120 billion annually.33 Thus, efforts to directly transform plastic waste into value-added products, such as polymeric membranes, is a step forward toward more sustainable industrial practices, specifically in the membrane industry.6,34,35
Several works have reported the successful utilization of plastic waste for membrane fabrication. Pulido et al.36 fabricated polyethylene terephthalate (PET) ultrafiltration membranes from plastic waste by NIPS, showing good performance even at temperatures up to 100 °C and high resistance towards harsh solvents. Lai et al.37 reported the use of polystyrene (PS) waste as a material source for fabricating waterproof CO2 separation membranes through hot-pressing. Keles and Uysal38 optimized the fabrication of low-density polyethylene (LDPE) and acrylic fiber membranes by electrospinning using shrink film packaging waste as the polymer source for wastewater treatment applications. These examples demonstrate the technical viability of using plastic waste as feedstock for membrane fabrication and the potential for environmental remediation.
In this work, we contribute to sustainability in polyolefin membrane fabrication through two approaches. First, by utilizing renewable bio-based solvents for PP and LDPE dissolution, and second, by implementing the direct recycling of plastic waste as a polymer source in the membrane fabrication process. The selected bio-based solvents were α-pinene and D-limonene, belonging to the terpene family, the largest class of natural products (produced by all plants), and have a long trajectory in human healthcare, with a FDA (U.S. Food and Drug Administration) approval for their use in food and cosmetics.39–42 They have been proposed as sustainable alternatives to fossil-derived solvents such as n-hexane for the extraction of valuable compounds, such as carotenoids, oil from seeds and microalgae, lipids, and aromas.43–45D-Limonene is produced from citrus fruits peels, a feedstock widely available from the juice industry waste, while α-pinene is derived from gum turpentine, an essential oil distilled from the pine gum harvested from living pine trees or obtained as a side product of the pulp mill industry (Fig. S1†).46,47 Their similar Hansen Solubility Parameters (HSP), compared to the petroleum-based p-xylene used in polyolefin dissolution, offers a great potential for their use as alternative greener solvents in PP and LDPE dissolution (Table S2†). Despite being renewable and widely available, their feasibility for polyolefin dissolution and membrane fabrication has not been studied to date, to the best of our knowledge. Here we proposed the use of α-pinene and D-limonene for polyolefin dissolution and membrane fabrication.
The phase diagrams were obtained from the solubility and phase separation mechanism of commercially available PP and LDPE in the bio-based solvents. Then, the effect of polymer content and quenching media on the PP membrane's morphology, mechanical and thermal properties, and water contact angle were addressed. The resulting membranes were tested in water-in-oil emulsion separation as an example of the application of hydrophobic PP membranes. Commercially available PP and plastic waste from PP food packages were utilized as the polymer source for membrane fabrication, and the changes in the membrane's properties and performance were investigated and compared.
This study broadens the alternatives for polyolefin (PP and LDPE) dissolution and membrane fabrication with renewable bio-based solvents while revalorizing plastic waste, which can be of benefit for the polymers and membrane fields in the transition to a circular economy following the green chemistry principles.
Ra2 = 4(δd2 − δd1)2 + (δp2 − δp1)2 + (δhb2 − δhb1)2 | (1) |
The phase diagrams were obtained by two methods: (i) observations of the dope solutions with different polymer contents on a Leica DM4500 P optical microscope and (ii) DSC measurements on a DSC 250 – TA instruments. The solutions were prepared in the same way for both methods. For optical microscopy observations, a drop of the polyolefin dope solution at 130 °C was placed between two glass slips with a 0.1 mm thickness at the same temperature and rapidly transferred into a Linkam Hot Stage, pre-heated at 140 °C. The temperature was maintained for five minutes and then decreased to room temperature (20 °C) at a 10 °C min−1 rate. The phase separation was observed during the cooling process under standard and polarized light. The cloud point (CP) was taken as the temperature at which the nucleus formation was observed with a 10× amplification lens.
DSC measurements were obtained by quenching the polyolefin dope solution with a specific composition in liquid nitrogen. A small piece of the solidified sample was then placed in a Tzero hermetic pan, heated to 140 °C and maintained for 20 min, cooled down to room temperature, kept for 10 min, and reheated to 140 °C to remove the thermal history of the polymer. Cooling–heating rates were 10 °C min−1 in all cases, and the exothermic peak temperature was taken as the crystallization temperature (Tc).
Thermal analysis was performed on a TGA Q50 instrument under an air atmosphere at a heating rate of 20 °C min−1 from 25 to 800 °C. DSC 250 and Tzero hermetic pans (TA instruments) were used for obtaining the crystallization and melting temperatures of polymers and PP membranes. In all cases, a heat–cool–heat cycle with an upper temperature of 230 °C was performed with a cooling–heating rate of 10 °C min−1.
SEM images were obtained on a Zeiss Merlin Electron Microscope. Samples for cross-section observations were prepared by breaking a piece of membrane in liquid nitrogen and placing it between two layers of conductive carbon tape. Silver paint was used on the borders of the membrane pieces to make contact between the carbon tape and the membrane. All samples were coated with a 3 nm iridium layer in a Quorum Q300RT sputter coater.
Water contact angles were measured on an FM40 Easy Drop instrument (KRÜSS). 2 μl water drop was utilized for air and under-oil measurements. All reported values are the average from three measurements.
Young's modulus, fracture strain, tensile strength, and toughness were obtained from strain vs. stress measurements on a Discovery DMA850 instrument. The stress ramp was set from 0.05 N to 18.00 N at a rate of 1.5 N min−1. Young's modulus was calculated as the slope of the linear section of the strain vs. stress curve; fracture strain was taken as the maximum strain value before the sample broke; tensile strength as the stress at which breaking occurred; and toughness was the area under the strain vs. stress curve. All reported values are the average from three measurements.
(2) |
(3) |
Solvent | Source | Boiling point | Solubility in water | Viscosity | Vapor pressure | Price |
---|---|---|---|---|---|---|
Bio/fossil | °C | mg L−1 | mPa s at 25 °C | mmHg at 25 °C | $ per kg | |
D-Limonene | Bio | 178 | 13.8 | 0.846 | 1.64 | 10 |
α-Pinene | Bio | 156 | 2.49 | 2.100 | 4.75 | 3 |
Benzene | Fossil | 80 | 1–5 | 0.654 | 76.00 | 0.8 |
Toluene | Fossil | 111 | 526 | 0.554 | 28.40 | 0.8 |
Chlorobenzene | Fossil | 132 | 0.5 | 0.806 | 12.00 | 0.8 |
Isooctane | Fossil | 99 | 2.2 | 0.473 | 49.30 | 2 |
p-Xylene | Fossil | 138 | 165 | 0.603 | 8.84 | 0.5 |
Trichloroethylene | Fossil | 87 | 1.28 | 0.545 | 69.00 | 0.5 |
Solvent | Source | Boiling point | Solubility in water | Viscosity | Vapor pressure | Price | CP | T c | References |
---|---|---|---|---|---|---|---|---|---|
Bio/fossil | °C | mg L−1 | mPa s at 25 °C | mmHg at 25 °C | $ per kg | °C | °C | ||
a Solvent mixed with 40 wt% carnauba wax. | |||||||||
α-Pinene | Bio | 156 | 2.49 | 2.1 | 4.75 | 3 | 74–88 | 46–65 | This work |
Soybean oil | Bio | — | — | 60.6 | — | 0.25 | 140–150a | ∼110 | Wang et al.23 |
Diphenyl ether | Fossil | 258 | 18 | 2.6 | 0.0225 | 5 | 137–115 | ∼97 | Yave et al.52 |
Dioctyl phthalate | Fossil | 384 | 0.022 | 39 | 2.6 × 10 × 10−6 | 1.5 | 152–162 | ∼107 | Yang et al.58 |
Diamyl phthalate | Fossil | 342 | 0.8 | No data available | 0.000196 | 277 | 193–177 | ∼107 | Lin et al.59 |
N,N-Bis(2-hydroxyethyl) tallowamine | Fossil | 269 | 1 × 10 × 106 | 351.9 | 2.8 × 10 × 10−4 | 0.6 | 157–147 | ∼104 | Lloyd et al.60 |
The PP used in this work was obtained from plastic waste containers or as commercially available PP pellets. For simplicity, the commercially available PP pellets are labelled as “pure PP”, and the one from plastic waste containers is referred to as “waste PP”. In both cases, for pure PP and waste PP, the FTIR spectra showed the characteristic peaks of C–H bending and stretching at 1375, 1455, and 2837–2950 cm−1 (Fig. S3†), and their fingerprint region was identical, confirming the absence of any organic polymer blend or organic additives in the material from the plastic containers (waste PP).
Once fully dissolved at 130 °C, the solution phase separation induced by temperature decrease was investigated by two different methods: (1) cloud point visual observation and (2) calorimetry (DSC). Similar phase separation behavior was observed for the three systems under study: pure PP in α-pinene, pure LDPE in α-pinene, and pure LDPE in D-limonene.
The cloud points (CP) or the visualization of the phase separation was possible by optical microscopy, as seen in Fig. 2, 3, S4, and S5.† The appearance of a second phase detected by optical microscopy without polarized light could result from a liquid–liquid (LL) or solid–liquid (SL) phase separation. The solid phase would arise by the crystallization of the polyolefin fraction. The use of polarized light and filters can distinguish the birefringent crystallized phase from amorphous liquid ones and therefore indicate the kind of phase separation (LL or SL). The crystalline phase is characterized by Maltese cross images typically seen in Fig. 2a, 3a, c and S5.†
Crystallization can be detected and quantified by calorimetric methods. DSC was conducted for the PP and LDPE systems with closed liquid panels and led to exact values of the crystallization temperature (Tc), which increased as the polymer content increased.51–54Fig. 1c and S6† show the crystallization curves for the polyolefin solutions and how the crystallization temperatures shift with the polymer concentration and the type of solvent. In the case of LDPE in α-pinene, the Tc ranged from 57.9 °C for 5 wt% polymer content to 72.6 °C for 35 wt%, while in D-limonene the Tc was 56.1 °C for 5 wt% and 75.4 °C for 40 wt% polymer contents. On the other hand, the Tc for pure PP in α-pinene ranged between 45.9 °C and 64.8 °C for 5 wt% and 25 wt%, respectively. In addition, from the DSC curves (Fig. S6†), the peak height and area increased with the increase in polymer content, denoting a larger enthalpy change in the three systems, correlated with the fraction of crystallizable material. The DSC of the waste PP in α-pinene (Fig. S7†) shows a broader crystallization curve with a peak shifted to higher temperature. This is probably mainly due to their differences in molecular weight and polydispersity (Table S2†).
From the optical microscopy observations and the calorimetric measurements, the phase diagrams depicted in Fig. 1d and 2e were obtained. A gap between curves obtained by the two methods was observed. This could indicate that first, as the temperature decreased, a liquid–liquid phase separation was initiated, with the generation of an amorphous polymer concentrated dispersed phase.13 As the temperature continued to decrease, the crystallization of the polymer concentrated phase was initiated as shown in the DSC analysis. As the crystallization proceeds, it can be seen also by the appearance of the birefringent Maltese crosses in the polarized optical microscope.
The crystallization or solid–liquid phase separation follows a nucleation and growth mechanism, which leads to the different final morphologies in the LDPE and PP systems (Fig. 3). In all PP concentrations, spherical structures (spherulites) with diameters around 35 μm were observed at the first stages of the phase separation process.
The phase-separated films prepared from LDPE using both solvents had poor mechanical properties and fell apart upon cooling. This can be related to the observed spherulitic morphology. The grain boundaries are weak points if the entanglement between them is not pronounced, which in this case could be related to the branched structure and low molar mass of LDPE (Table S3†). For this reason, the membrane preparation and performance were focused on the PP in the α-pinene system only, which led to membranes with higher mechanical stability.
The solubility of polyolefins demonstrated hereby could be useful for coatings, recycling, and any other application requiring a solution process, which typically rely on fossil-based solvents, some of them possessing carcinogenicity or reproductive toxicity.55–57 Besides the advantage of D-limonene and α-pinene of being bio-based and renewable, they are more sustainable options against traditional solvents used for polyolefin solubilization, as shown in Table 1. Their solubility in water is lower than that for toluene and p-xylene, and their vapor pressure is lower than those of all other listed solvents, implying a lower exposure to vapors for people working with them. Based on these characteristics, the solvent recovery of the bio-based solvents can be done via rotavapor evaporation of the ethanol from the solvent exchange step after the membrane preparation (Fig. S15†).
The viscosity of D-limonene at room temperature is close to those of the fossil-based solvents, which implies that transporting and handling in a process would not require a large amount of extra energy. However, for industrial scale exploitation of D-limonene, its price needs to be lower than that as of today.
To better assess the benefits of α-pinene specifically for PP membrane fabrication, a comparison of α-pinene with other solvents reported for PP membrane fabrication via TIPS is shown in Table 2. As TIPS is driven by a temperature change, the cloud points and crystallization temperatures are of main importance in terms of energy consumption. As can be observed, α-pinene allows PP membrane formation at lower temperatures, and therefore results in lower energy requirements. Its lower viscosity could be advantageous in terms of processing, and its lower boiling point could facilitate its recovery. It can also be noticed that its price is competitive against other solvents used for PP membrane fabrication. Thus, α-pinene represents a good alternative for PP membrane fabrication.
Passive cooling of the polymer solution on the steel plate by contact with air allowed a slow temperature decrease. By immersing the plate in water, the temperature decreased much faster. The water thermal conductivity is 0.6 W m−1 K−1, while that of air is 0.025 W m−1 K−1, which is 20 times smaller. Cooling is even faster when the water is at 4 °C.
Water and both solvents are practically immiscible. The solubility of α-pinene and D-limonene in water is 2.5 mg L−1 and 13.8 mg L−1, and their boiling points are around 157 °C and 176 °C, respectively. Therefore, there was practically no solvent evaporation, and the solvent–water exchange was negligible. In the subsequent fabrication step, an effective exchange occurred when the film was immersed in ethanol (Fig. 1).
The effect of polymer content and quenching media on the membrane morphology was analyzed using surface and cross-sectional SEM micrographs. The PP membranes prepared with α-pinene as the solvent featured spherulitic structures with varying size depending on the polymer content and quenching media (Fig. 4). At polymer contents below the critical concentration, phase separation occurs by nucleus formation and growth of a spherical polymer-rich region. After the phase separation, as the spherical nuclei grow, they become interconnected and solidify, forming the membrane structure, and the surrounding polymer-lean space becomes the membrane's pores.61 This is the case for the PP in the α-pinene system.
For the membranes quenched in air (Fig. 4a, d, and g), the surface morphology remained similar when varying the PP content, with the spherulite size ranging between approximately 20 and 30 μm, and no visible pores. On the other hand, the use of water at 20 °C as quenching medium limited the spherulite growth (Fig. 4b, e, and h), leading to sizes around 15, 4, and 3 μm for 15, 20, and 25 wt% polymer content, respectively. Lowering the water temperature to 4 °C considerably reduced the spherulite size for all three concentrations (Fig. 4c, f, and i). For 15 wt% polymer content, it reduced to 0.7 μm; for 20 wt%, to 0.5 μm; and for 25 wt%, to a size too small to be measured under the given amplification. Such size reduction can be related to the degree of supercooling ΔT (Tm − T) associated with the use of each quenching medium. According to the polymer crystallization theory, the critical lamella size for crystallization to start is inversely proportional to the supercooling of a polymer solution.62 This implies that at the lowest temperature of the quenching media (in this case, water at 4 °C), the critical lamella size is smaller, and more nuclei can be formed. Similar conclusions can be made concerning the effect of polymer content. Higher polymer content solutions exhibited a higher Tm (Fig. S6†), and thus, a larger ΔT is applied when quenching compared with lower polymer contents. This also resulted in a larger number of nuclei for higher polymer contents (Fig. 3). These variations in the critical lamella size and the number of nuclei formed led to the observed spherulite size reduction with the increase in polymer content and the decrease in the quenching medium temperature.
The cross-sectional SEM micrographs shown in Fig. 4j–l confirmed that the use of α-pinene as a solvent resulted in the formation of PP spherulites across the membrane's internal structure. The structure is asymmetric, which can be explained by the different cooling rates of the top and bottom layers. Due to the fabrication method followed in this work, the top of the membranes was directly in contact with the quenching media, while the metallic plate added thermal resistance for the bottom to cool down. This phenomenon has been observed in other PP–solvent systems.63 The five minutes quenching conditions have a strong influence on the morphology. The immersion in water with 20 times higher thermal conductivity rapidly brought the system to the phase separation temperature and promoted fast growth of spherulites. At the time that the film was immersed in ethanol, the membrane formation was practically complete. Films quenched in air demonstrated a denser morphology. We hypothesize that upon immersion in ethanol, the film was not completely solidified yet, and the solvent diffused into the ethanol bath, which resulted in a denser and thinner film.
The results from strain vs. stress measurements showed a strong dependency between mechanical properties and the quenching media for the pure PP membranes, while the effect of polymer content was more noticeable on the membrane's toughness (Fig. 5 and Table S4†). Membranes prepared with 15 wt% polymer content and quenched in water at 20 °C had inferior mechanical properties and could not be tested.
Among all tested membranes, Young's modulus and tensile strength were higher for membranes quenched in air at 20 °C (Fig. 5), denoting a larger linear elastic region that can be associated with the denser internal structure observed by SEM. However, the same membranes had lower fracture strain and toughness. In these two aspects, membranes quenched in water at 4 °C had higher values. This can be associated with the dense structure of the membranes quenched in air.
Compared to other PP membranes reported in the literature with spongelike or cellular structures, the membranes obtained in this work had lower mechanical properties.23,64 Thus, it can be assumed that the PP membrane spherulitic morphology significantly affects their mechanical properties. A similar conclusion was reported for membranes prepared with poly(vinylidene fluoride) (PVDF), another aliphatic semicrystalline polymer.65 In their study, the same material had very different mechanical properties depending on the final morphology of the membrane, the highest for interconnected cellular structures and the lowest for interconnected globules. Thus, the same situation could occur for the PP membranes obtained in this work.
Slight differences in the melting and crystallization temperatures were observed after the film preparation using different quenching conditions (Fig. S8†). The Tm decreased from 167 °C to 162 °C, while the Tc remained close to the original value of 118 °C except for the membrane quenched in water at 20 °C, which increased to 119 °C. The crystallization and melting enthalpies of the prepared membranes varied less than 5% compared to the pure original polymer pellets, denoting a similar degree of crystallinity. Similar results were obtained with all polymer contents (Fig. S8 and Tables S5, S6†).
All prepared films were highly hydrophobic, with water contact angles of approximately 100° (Fig. S10†), as expected for PP films.68,69 Films quenched in water at 20 °C were the most hydrophobic. Surface roughness can increase the water contact angle by inducing a Cassie state,70 which might contribute to the higher values for those films due to their rougher surfaces. The membranes prepared from 20 and 25 wt% pure PP solutions exhibited under-oil (in hexane, heptane, and toluene) water contact angles above 150° (Fig. S11†), classifying them as under-oil superhydrophobic and indicating their suitability for water-in-oil emulsion separation.
Based on the selection of pure PP membranes, similar conditions were applied to fabricate membranes from PP plastic waste as the polymer source. The dope solution of waste PP had a lower viscosity than that of commercial pure PP solution.
This difference can be attributed to its lower molecular weight (Table S2†), which also lowered the mechanical properties of the final waste PP membranes compared with the ones prepared from pure PP pellets under the same conditions (Table S4†). Thus, higher waste PP polymer content was able to be dissolved at the same temperature as pure PP (130 °C), resulting in mechanically stable membranes that were successfully tested for the separation process. Waste PP concentrations that allowed membrane formation were between 25 and 30 wt%. Quenching in water at 4 °C led to membranes with the best mechanical stability up to 18 MPa for 30 wt% waste PP (Fig. S12c and d†). SEM images revealed a surface and cross-section spherulitic morphology like those of pure PP membranes, with an asymmetric structure (Fig. S13†), and similar under-oil water contact angles above 150° (Fig. S12†).
The thermal properties of the waste PP membranes were compared with those of the membranes prepared from commercial PP pellets (Fig. S14†). The TGA curves showed that 90% of the waste PP membrane weight is lost at around 350 °C, lower than the 376 °C observed for pure PP. In the case of melting and crystallization behavior, the DSC curves showed a lower Tm of 161 °C and a higher Tc of 123 °C compared to the pure PP pellets (Tm of 167 °C and Tc of 118 °C).
After an initial heptane filtration test performed with mechanically stable membranes (Table 3), six fabrication conditions for PP membranes were chosen for further testing. Filtration tests of selected membranes were performed for n-heptane, n-hexane, and toluene (Fig. 6). The permeance was lower for higher polymer content and decreased with the hydrocarbon viscosity. In the case of pure PP membranes, lower permeance was observed for membranes with higher polymer content, which can be associated with smaller pore size, as observed by SEM. The permeance was the highest for n-hexane, the hydrocarbon with the lowest viscosity (Table S1†), ranging from 0.28 to 0.7 L m−2 h−1 bar−1, followed by heptane and toluene with 0.25 to 0.56 and 0.22 to 0.48 L m−2 h−1 bar−1, respectively.
Fig. 6 Pure and waste PP membrane performance: (a) hydrocarbon permeance and (b) water rejection in the separation of water in toluene emulsion. |
Sample | PP source | Polymer content (wt%) | Quenching media | Heptane permeance (L m−2 h−1 bar−1) |
---|---|---|---|---|
20%_4 °C | Pure | 20 | Water at 4 °C | 0.69 |
22.5%_4 °C | Pure | 22.5 | Water at 4 °C | 0.44 |
25%_4 °C | Pure | 25 | Water at 4 °C | 0.00 |
22.5%_20 °C | Pure | 22.5 | Water at 20 °C | 0.61 |
25%_20 °C | Pure | 25 | Water at 20 °C | 0.28 |
W25%_4 °C | Waste | 25 | Water at 4 °C | 0.30 |
W27.5%_4 °C | Waste | 27.5 | Water at 4 °C | 0.32 |
W30%_4 °C | Waste | 30 | Water at 4 °C | 0.06 |
The permeance of membranes prepared from waste PP membranes was practically independent of the dope solution polymer content, since the upper layer morphologies of the membranes prepared from 25 and 30 wt% were similar (Fig. S13†).
All membranes demonstrated a good separation performance for water-in-toluene emulsions (Fig. 6). The two best performing pure PP membranes (22.5 wt% PP quenched in water at 20 °C and 25 wt% when quenched at 20 °C) demonstrated 95.7% water rejection, while both tested waste PP membranes had rejections of 95.0% and 94.9%. These results imply around 99.97% toluene purity in terms of water content. All obtained permeance, water rejection, and water content in the permeate values are shown in Table S7.† From DLS measurements, it was observed that the water drops in the emulsion had diameters above 200 nm.
Comparable toluene purity values have been reported by other hydrophobic membranes.50,68,69,71 Tao et al.50 reported a toluene purity of 99.96% after the filtration of a water-in-toluene emulsion with 1% water content utilizing a modified PVDF membrane. Kansara et al.69 prepared superhydrophobic membranes by coating alkylsiloxane-silica nanoparticles on a PP fabric and obtained a toluene purity above 99% from a 10% water containing water-in-toluene emulsion.
The use of renewable bio-based solvents and plastic waste reported in this work represents a greener and more straightforward method to fabricate PP membranes for water-in-oil emulsion separation.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2gc03181g |
‡ These authors contributed equally to this work. |