Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Catalytically active nanosized Pd9Te4 (telluropalladinite) and PdTe (kotulskite) alloys: first precursor-architecture controlled synthesis using palladium complexes of organotellurium compounds as single source precursors

Aayushi Aroraa, Preeti Oswala, Gyandshwar K. Raob, Sushil Kumara, Ajai K. Singhc and Arun Kumar*a
aDepartment of Chemistry, School of Physical Sciences, Doon University, Dehradun, Uttarakhand 248012, India. E-mail: arunkaushik@gmail.com; akumar.ch@doonuniversity.ac.in
bDepartment of Chemistry, Amity School of Applied Sciences, Amity University Haryana (AUH), Gurgaon, Haryana 122413, India
cDepartment of Chemistry, Indian Institute of Technology Delhi, New Delhi, 110016, India

Received 13th October 2020 , Accepted 7th January 2021

First published on 11th February 2021


Abstract

Several intermetallic binary phases of Pd–Te including Pd3Te2, PdTe, PdTe2, Pd9Te4, Pd3Te, Pd2Te, Pd20Te7, Pd8Te3, Pd7Te2, Pd7Te3, Pd4Te and Pd17Te4 are known, and negligible work (except few studies on PdTe) has been done on exploring applications of such phases and their fabrication at nanoscale. Hence, Pd(II) complexes Pd(L1)Cl2 and Pd(L2-H)Cl (L1): Ph–Te–CH2–CH2–NH2 and L2: HO–2-C6H4–CH[double bond, length as m-dash]N–CH2CH2–Te–Ph were synthesized. Under similar thermolytic conditions, complex Pd(L1)Cl2 with bidentate coordination mode of ligand provided nanostructures of Pd9Te4 (telluropalladinite) whereas Pd(L2-H)Cl with tridentate coordination mode of ligand yielded PdTe (kotulskite). Bimetallic alloy nanostructures possess high catalytic potential for Suzuki coupling of aryl chlorides, and reduction of 4-nitrophenol. They are also recyclable upto six reaction cycles in Suzuki coupling.


Introduction

Materials at nanoscale possess new and improved properties compared to their bulk counterparts. Hence, the scientific community has focused its attention on the fabrication of nanosized materials.1 Composition, stability, size and shape are among those factors on which the physicochemical properties of nanomaterials have been found to depend.1 In this regard, metal chalcogenide nanomaterials1–3 have attracted the attention of researchers increasingly due to their various applications in energy conversion, storage and electronics,2–5 development of materials for semiconductors,6–8 dye-sensitized solar cells,9,10 magnesium–air batteries,11 aerogel fabrication,12 and catalysis.13–20

Among different metal chalcogenides reported in literature, significant work has been done in recent past on the exploration and development of binary phases of tellurides of various metals (excluding palladium), mainly due to their potential application2 in memory devices, photovoltaic cells, thermoelectrics, biochemical applications, semiconductors with enhanced thermoelectric properties in nanocomposites, photothermal therapy, thin films and nanomaterials and catalysis.2,4,18–20 After the discovery of easy methods of preparation16,17,21 of binary phases of palladium selenide and their role in catalysis,16,17 there has been an enormous increase during last five years on the discovery of interesting applications of palladium selenides3,9–14 in various fields including catalysis. Binary phases of palladium tellurides are also envisaged to be among applied nanomaterials. Binary phases reported so far include PdTe, Pd3Te2, PdTe2, Pd9Te4, Pd2.5Te, Pd3Te, Pd2Te, Pd20Te7, Pd8Te3, Pd7Te2, Pd7Te3, Pd4Te and Pd17Te4.22 Among such phases, only PdTe,18–20 Pd20Te27 (ref. 23) and Pd13Te3 (ref. 24) have been studied upto some extent. Catalysis, an important applications of other metal chalcogenides, has not seen the potential of binary phases of palladium tellurides except a few reports on PdTe.18–20

Pd9Te4 (telluropalladinite), an intermetallic system, is a palladium rich binary phase which was reported by Matkovic and Schubert for the first time in year 1978.25 Only a little is known and reported about this material.25,26 Its crystal structure25 and phase relations26 has been studied. To the best of our knowledge, laboratory synthesis for its bulk material is rarely investigated, and its fabrication at nanoscale and potential applications have not yet been investigated.

A convenient route to produce metal chalcogenide materials is by thermal decomposition6,7 of single source precursors (SSP) i.e. metal complexes containing organochalcogen ligands. This route has advantages over the conventional methods as it does not require distinct sources for palladium and chalcogen, sophisticated equipments and extremely high temperature. Since molecules of only a single precursor are available in the reaction vessel in SSP route, reaction handling becomes easy and the possibility of occurrence of pre-reaction and contamination is minimized. The work-up procedures are also simple due to easy removal of organic by-products by filtration or centrifugation. Some metal complexes (except those of Pd and Pt) of tellurium ligands have been used as SSPs for the synthesis of nanosized binary tellurides (such as Sb3Te2, SnTe, PbTe, ZnTe and CdTe) of different metals.2,6,8 Though the ligand chemistry of organotellurium compounds is explicitly explored with palladium and a variety of coordination compounds have been synthesised,6,8 use of such compounds as SSPs for the development of nanostructures of binary phases of palladium tellurides at bulk or nano-scale have been rarely explored.24 However, in situ generation of Pd3Te2 nanoparticles has been reported during catalysis of a Suzuki–Miyaura coupling by a tellurium ligated molecular Pd(II) complex.

It is worth noting that (i) a little has been studied and reported about most of the binary phases of palladium tellurides including Pd9Te4 which has not been fabricated at nanoscale so far and not explored for applications, (ii) there are only a few reports on the synthesis of PdTe nanocrystals, (iii) molecular architecture of precursor plays a significant role in determining the composition and/or morphology of nanostructures in SSP route,1,17,27 (iv) applications of binary phases of palladium tellurides are rarely explored in catalysis, and (v) when dispersion of nano-scale palladium tellurides continues to decrease and reaches the single atom limit, it may become a single-atom catalyst. Such single atom catalysts are expected to obtain better catalytic activity and efficiency.28–31 It is, therefore, thought to develop a SSP based easy route for the precursor-architecture controlled synthesis of PdTe and Pd9Te4 nanostructures, and to carry out the screening of their catalytic potential for Suzuki coupling of chloroarenes and reduction of 4-nitrophenol, the chemical transformations of immense utilities.32,33

In the present work, the ligands L1, L2 and their Pd(II) complexes 1 and 2 have been synthesized. The major structural difference between 1 and 2 is the coordination mode (Fig. 1 and 2) of ligand (i.e. bidentate in 1 and tridentate in 2). The 1 and 2 have been used as designers single source precursors to obtain nanoparticles of different alloys (Pd9Te4 from 1 and PdTe from 2) under similar conditions of thermolysis. Both the nanosized alloys show a high potential for catalysis of Suzuki coupling and reduction of nitroarenes.


image file: d0ra08732g-f1.tif
Fig. 1 ORTEP diagram of complex 1 with 50% thermal ellipsoids. Selected bond lengths (Å): Te–Pd: 2.5057(6), Te–Caryl: 2.118(6), Te–Calkyl: 2.149(6), Pd–Cl: 2.3142(16), Pd–Cl; Pd–N: 2.063(5). Selected bond angles (°): Cl–Pd–Te: 88.82(4), Cl–Pd–Cl: 94.42(6), N–Pd–Te: 88.21(13), N–Pd–Cl: 88.54(14).

image file: d0ra08732g-f2.tif
Fig. 2 ORTEP diagram of complex 2 with 50% thermal ellipsoids. Selected bond lengths (Å): Te–Pd: 2.5002(4), Te–C: 2.120(4), Pd–Cl: 2.3271(11), Pd–O: 2.007(3), Pd–N: 2.017(4). Selected bond angles (°): Cl–Pd–Te: 86.74(3), O–Pd–Cl: 88.98(9), N–Pd–Te: 90.94(10), N–Pd–O: 93.18(13).

As an enormous surge in the investigations on interesting applications of binary phases (such as Pd17Se15, Pd4Se and Pd7Se4) of palladium selenide has been noticed after year 2015,3,9–14 the results of this report open up a field for development of nanostructures of several binary phases of palladium telluride using easy methods involving deployment of SSPs and controlling the compositions as well as physicochemical properties of NPs simply by using tailor-made organotellurium compounds. Additionally, it is also a promising beginning for applications of new alloy (Pd9Te4) in the field of catalysis followed by other fields such as electrocatalysis, oxygen reduction reactions, etc.

Results and discussion

Syntheses and characterization

The L2, 1 and 2 have been prepared (Scheme 1) and characterized with 1H, 13C and 125Te NMR spectroscopy (ESI: Fig. S1–S8) and mass spectrometry (ESI: Fig. S9 and S10). Molecular structures of 1 and 2 have also been authenticated (Fig. 1 and 2) using single crystal X-ray diffraction studies. 125Te nuclei are NMR active and very sensitive to their local electronic environment. A minor change in such an environment leads to significant changes in chemical shift positions in 125Te NMR spectroscopy. Similar phenomenon is observed with chemical shift position of the signal of free ligand L2. This signal undergoes a deshielding of 864 ppm when L2 is transformed into complex 2. It happens due to decrease in electron density around nucleus of Te by virtue of the involvement of tellurium in the formation of a coordination bond with palladium. Single crystal X-ray diffraction studies also revealed the existence of such a bond between Te and Pd in complex 1 as well as 2. Both the complexes exhibit a square planar geometry (Table 1) around the palladium centre. The ligand binds in a bidentate mode in 1 (Fig. 1) and tridentate mode in 2 (Fig. 2). In complex 2, the Pd–Cl bond (trans to nitrogen donor) is slightly longer [2.3271(11) Å] than the one [2.3142(16) Å] in complex 1. This Pd–Cl bond length in the 1 is consistent with the literature reports.34 The Pd–Te bond length in both the complexes are similar i.e. 2.5057(6) and 2.5002(4) Å in complexes 1 and 2 respectively. The Pd–O bond length in complex 2 is 2.007(3) Å. These bond lengths are in agreement with the earlier reports.35,36 The Caryl–Te bond length [2.118(6) Å] is slightly shorter than Calkyl–Te bond length [2.149(6) Å].35,36
image file: d0ra08732g-s1.tif
Scheme 1 Strategy for syntheses and catalytic reactions.
Table 1 Crystal data and structural refinement parameters of complexes 1 and 2
Parameters 1 2
Formula C8H11Cl2NPdTe C16H16ClNOPdTe
Formula weight (g mol−1) 426.08 507.75
Color Yellow Orange
Space group [P with combining macron]1 P21/n
Temperature/K 293(2) 150.00(10)
λ (Å) (Cu-Kα) 0.71073 0.71073
Crystal system Triclinic Monoclinic
a (Å) 7.9097(8) 16.7218(2)
b (Å) 8.4514(10) 19.2440(3)
c (Å) 8.85568(7) 20.2510(3)
α (°) 83.934(8) 90
β (°) 87.438(8) 99.6590(10)
γ (°) 86.644(9) 90
V3) 567.27(10) 6424.28
Z 2 16
ρcalc (g cm−3) 1.083 2.099
F(000) 396 3872
Theta range for data collection 2.395 < θ < 28.123 2.0240 < θ < 28.0940
Index ranges −8 < h < 10 −21 < h < 22
−11 < k < 10 −24 < k < 25
−9 < l < 11 −11 < l < 27
GOF on F2 1.059 1.0263
R1 [I > 2σ(I)] 0.0478 0.0446
R1 [all data] 0.0355 0.0332
wR2 [I > 2σ(I)] 0.0725 0.0749
wR2 [all data] 0.0821 0.0855
CCDC 1[thin space (1/6-em)]994[thin space (1/6-em)]616 1[thin space (1/6-em)]994[thin space (1/6-em)]615


Before subjecting complexes 1 and 2 to thermolysis, their thermal decomposition temperatures have been determined using thermogravimetric analysis. Such a decomposition occurred at 260 °C in case of complex 1, and at 240 °C in case of 2, with a weight loss of 30% and 50% respectively [Fig. 3(a) and (b)]. Hence, both the complexes were used as new single source precursors (SSP) and pyrolyzed (Scheme 1) at 260 °C and 240 °C in a mixture (1[thin space (1/6-em)]:[thin space (1/6-em)]1) of oleyl amine and oleic acid. This led to the formation of nanostructures of Pd9Te4 (from complex 1) and PdTe (from complex 2). The nanostructures have been characterized by FTIR, PXRD, SEM-EDX, TEM, DLS, BET and XPS techniques. In the FTIR spectra, the bands due to the presence of stabilizer molecules of oleyl amine and oleic acid are visible in case of both the nanostructures. The IR spectrum of Pd9Te4 [Fig. 4(a)] exhibits absorption bands at 2920 and 2844 cm−1 due to symmetric and asymmetric stretching vibrations of the aliphatic –CH2 group. Similar bands are observed at 2914 and 2855 cm−1 in PdTe [Fig. 3(b)]. The bands at 1627 and 1694 cm−1 in Pd9Te4 and PdTe may be attributed to the C[double bond, length as m-dash]O vibrations. NH2 bending vibrations [Fig. 4(a) and (b)] are likely to be represented by the bands at 1527 cm−1 in Pd9Te4 and 1554 cm−1 in PdTe. The absorption bands at 1436, 1099 and 672 cm−1 are likely to correspond bending vibrations of CH3, C–N and C–C bonds respectively.37,38


image file: d0ra08732g-f3.tif
Fig. 3 TGA curves of (a) complex 1 (b) complex 2.

image file: d0ra08732g-f4.tif
Fig. 4 FTIR spectra of (a) Pd9Te4 (b) PdTe nanostructures.

The PXRD pattern of Pd9Te4 [Fig. 5(a)] reveals a monoclinic structure when matched with standard phases (JCPDS # 34-1359). The PXRD pattern of NPs 2 [Fig. 5(b)] corroborates the presence of a hexagonal PdTe phase (JCPDS # 29-0971). PXRD patterns are sharp. Such patterns do not indicate presence of any impurity as any high intensity peaks which do not belong to the phase of the material are absent. The results of the SEM-EDX studies [Fig. 6(a) and (b)] are in good agreement with the data obtained from the PXRD pattern.


image file: d0ra08732g-f5.tif
Fig. 5 PXRD spectra of (a) Pd9Te4 (b) PdTe nanostructures.

image file: d0ra08732g-f6.tif
Fig. 6 SEM-EDS spectra of (a) Pd9Te4 (b) PdTe nanostructures.

The morphologies of both the nanostructures have been studied using High Resolution Transmission Electron Microscopy (HRTEM) (Fig. 7). Theses nanostructures of Pd9Te4 and PdTe (obtained from complexes 1 and 2) appear to be spherical in shape. HRTEM images also corroborate uniform distribution of nanoparticles with size of 10–25 nm in both the cases.


image file: d0ra08732g-f7.tif
Fig. 7 HRTEM images of nanostructures of Pd9Te4 (a and c) and PdTe (b and d).

Dynamic light scattering (DLS) studies have also been performed in order to understand the particle size distribution. During such studies, the particles moves with the added solvent or stabilizer. It is well known that DLS provides information about hydrodynamic diameter (diameter of particle with hydration shell).39,40 This diameter corresponds to the collective form of particle and stabilizer or solvent. In the present study, the hydrodynamic diameter has been found to be 106 and 220 nm for Pd9Te4 and PdTe NPs [Fig. 8(a) and (b)]. However, the molecules of the stabilizers (oleyl amine and oleic acid) are not diagnosed in the HRTEM studies as they are electron transparent. The presence of molecules of oleyl amine and oleic acid (that act as stabilizers) in the hydration shell is the most probable reason for the difference in the size, revealed by the two techniques HRTEM and DLS.41 The value of polydispersity index (PDI) has been found to be 0.336 (below 0.5) suggesting the high colloidal stability and low sedimentation potential. It is also known from Rayleigh's approximation that the intensity of the scattering of particles is proportional to the sixth power of the diameter i.e. I = d6. Therefore, the DLS results are influenced by the presence of larger particles even if they are very less in number (Table 2).40


image file: d0ra08732g-f8.tif
Fig. 8 DLS analysis of (a) Pd9Te4 and (b) PdTe nanostructures.
Table 2 Particle size distribution of Pd9Te4 and PdTe nanostructures
Pd9Te4 nanostructures
Size (d. nm) 91.3 106 122 142.5
Intensity (%) 19.7 44.7 30.3 5.3
PdTe nanostructures
Size (d. nm) 112.5 150 220 295.5
Intensity(%) 10.3 35.3 39.7 14.7


The XPS spectral information has been used to elucidate the valence distribution of palladium (Fig. 9) and tellurium (ESI: Fig. S13 and S14) atoms. The binding energies of both Pd-3d region and Te-3d region are given in Table S3. Analysis of high-resolution spectrum in the binding energy region of Pd-3d in Pd9Te4 (Fig. 9) shows the presence of two sets of peaks in the Pd-3d region (336.06 eV, 341.39 eV and 337.80, 343.08 eV). The enlarged spectra of PdTe (Fig. 9) also indicated the Pd-3d peaks in the similar binding energy region (337.80 eV and 343.08 eV).


image file: d0ra08732g-f9.tif
Fig. 9 XPS spectra of (a) Pd9Te4 and (b) PdTe nanostructures.

The positive shift in both the cases is attributed to the higher donation of electrons from Te to Pd centre in PdTe. Interestingly, there is a drift towards Pd(0) values as the palladium content in the phase is increased (from PdTe to Pd9Te4). The 3d spectra of Te (Fig. S14) also reflect a doublet corresponding to 3d5/2 and 3d3/2 in Pd9Te4 (573.60 and 582.50 eV) and PdTe (374.29 eV and 583.10). Hence, the presence of both Pd(0) and Pd(II) species on the surface of both the nanostructures is indicated (details in ESI). The surface area and pore volume were also calculated using N2 adsorption–desorption insotherm (Fig. 10). The BET surface areas have been found to be 18.424 m2 g−1 and 4.9565 m2 g−1 for Pd9Te4 and PdTe nanostructures respectively. The average pore size was found to be less than 2 nm in both the cases, suggesting the presence of only micropores. The pore volume was calculated and found to be 0.033 and 0.008 cm3 g−1 indicating that these are non-porous materials. These materials exhibit a type IV hysteresis loop that is observed when the substances have micropores and mesopores.42


image file: d0ra08732g-f10.tif
Fig. 10 N2 adsorption–desorption isotherm of Pd9Te4 and PdTe nanostructures.

Catalytic studies

The catalytic potential of both the nanostructures has been evaluated (Table 3) for Suzuki Miyaura C–C coupling (Scheme 1) of chloroarenes. These substrates were chosen for the study because aryl chlorides have easy availability. In addition, they suffer from the lowest reactivity among haloarenes (ArI, ArBr and ArCl). In case of coupling of such substrates, the palladium-based catalysts must be able to overcome the high activation barriers of the substrates. Hence, presence of electron rich active sites is desired in most homogeneous palladium catalysts. Such sites are generated by the presence of electron-donating ligands. However, the use of palladium complexes and ligands is generally avoided in chemical industry due to their high cost and toxicity. In contrast, heterogeneous catalysts, which offer the advantage of their facile reusability and compatibility with flow systems, are preferred. In such catalytic systems, high activity and stability require negatively charged or electron rich Pd species with negligible metal leaching or clustering. In this context, in recent past, nanosized bimetallic alloys have attracted attention of the researchers as they show improved catalytic activity than monometallic catalysts, at nanoscale, due to the electronic and geometrical modifications which arise as a consequence of synergic cooperation between the two metals of alloys.43–50 In the present study, both Pd9Te4 and PdTe are bimetallic alloys in which active Pd atoms are incorporated in a lattice together with Te.25,26 Hence, these intermetallic phases are likely to offer the advantage of hosting solid active sites. In addition, Pd9Te4 has a higher valence electron concentration26 which may play a role in generating electron rich palladium species.
Table 3 Results of catalysis Suzuki coupling between aryl chlorides and phenylboronic acid by nanostructures of Pd9Te4 and PdTea
S. no Substrate % conversion (NPs 1) % conversion (NPs 2)
a Reaction conditions: aryl chloride (1.0 mmol), phenylboronic acid (1.1 mmol), K2CO3 (2.0 mmol), catalyst 5.0 mg, time 12 h, temperature 100 °C.
[1] 4-Chlorobenzaldehyde 88 87
[2] 4-Chloronitrobenzene 85 83
[3] 4-Chloroacetophenone 79 78
[4] 4-Chlorobenzonitrile 85 84
[5] Chlorobenzene 82 80


Before conducting catalytic studies on the nanosized PdTe and Pd9Te4, reaction conditions and parameters were optimized. Such parameters include use of K2CO3 as a base, and aqueous DMF (DMF[thin space (1/6-em)]:[thin space (1/6-em)]Water = 1[thin space (1/6-em)]:[thin space (1/6-em)]1) (ESI: Table S4, entry 2) as solvent system.

Coupling reactions of all the aryl chlorides (i.e. 4-chlorobenzaldehyde, 4-chloronitrobenzene, 4-chloroacetophenone, 4-chlorobenzonitrile and chlorobenzene) were carried out and studied at these optimized reaction conditions. All the substrates gave comparable yields of cross-coupled products. 4-Chlorobenzaldehyde was converted to 4-biphenylcarboxaldehyde in 88% and 87% conversion when NPs of Pd9Te4 and PdTe (5.0 mg) were used as a catalyst in 12 hours (Table 3, entry 1). The conversion of the substrates into the products, observed in the reactions of 4-chloronitrobenzene and 4-chlorobenzonitrile, were 85% when Pd9Te4 was used as a catalyst (Table 3, entry 2, 4). However, when nanocatalyst PdTe was employed, a marginally decrease was observed, and % conversions were found to be 83% and 84% respectively (Table 3, entry 2, 4). Other substrates (i.e. 4-chloroacetophenone and chlorobenzene) also gave good (i.e. ≥78%) conversions. Hence, it may be inferred that nanoparticles of palladium rich phase Pd9Te4 are slightly more efficient than those of PdTe.

The number of catalytic systems in general and nanocatalytic systems in particular, which are competent to catalyze the coupling of aryl chlorides, is not very high.51–63 In fact, aryl chlorides are the least reactive substrates, and most of the catalytic systems either show inactivity for these substrates or show very low efficiency. Many of the reported palladium based nanocatalytic systems require longer reaction times (Table 4, entry 2, 4)53,55 and/or give lower conversions (Table 4, entry 1, 3, 15)52,54,63 in comparison to our Pd9Te4 and PdTe nanocatalysts. However, some of them are able to operate in EtOH/H2O (Table 4, entry 1–4, 15).52–55,63

Table 4 Performance of known palladium based nanocatalytic systems for Suzuki coupling between chlorobenzene and PhB(OH)2

image file: d0ra08732g-u1.tif

Entry no. Catalyst Solvent Catalyst amount Time (h) Temp (°) % conversion Ref.
a 4-Bromobenzaldehyde.b 4-Chlorobenzaldehyde.c 1-Bromo-4-nitrobenzene.
[1] Pd1Ni4/CNF EtOH/H2O 5 mg 5 80 7 52
[2] Isoniazide-MWCNTs-Pd EtOH/H2O 14 mg 24 60 70 53
[3] Chitosan-biguanidine/Pd EtOH/H2O 10 mg 10 40 70 54
[4] MWCNTs/CC-SH/Pd EtOH/H2O 10 mg 24 80 70 55
[5] Pd NPs@PPh2-SiO2 DMF 0.5 mol% 5 100 95 56
[6]a Pd3Te2 Aq. DMF 2 mol% 15 100 86 57
[7] Pd(0) NPs (stabilized by bulky organosulphur ligand) Aq. DMF 3 mg 3 100 45 58
[8]b Pd(0) NPs (stabilized by anthracene-based organosulphur ligand) Aq. DMF 5 mg 12 100 75 59
[9]b Pd(0) NPs (stabilized with anthracene based organoselenium ligand) Aq. DMF 5 mg 12 100 84 59
[10]b Pd(0) NPs (stabilized with didocosyl selenide) Aq. DMF 5 mol% 24 100 32 60
[11] PdS Aq. DMF 5 mg 12 90 78 61
[12] Pd16S7 Aq. DMF 5 mg 12 90 74 61
[13]c Pd16S7 Aq. DMF 0.1 mol% 24 100 88 62
[14]c Pd16S7 Aq. DMF 0.1 mol% 24 100 81 62
[15] Pd@AGPO EtOH/H2O 5 mg 6 80 25 63
[16] Pd9Te4 Aq. DMF 5 mg 12 100 84 Present work
[17] PdTe Aq. DMF 5 mg 12 100 82 Present work


Reports about the use of nanosized alloys of palladium as catalysts of Suzuki coupling are rare, but not non-existent in the literature. Such alloys include Pd1Ni4, CuPd, Y3Pd2, Pd3Te2 and Pd17Se15.43,48,52,57,64 The alloy Pd1Ni4 has been grafted on carbon nanofibers and the resulting system (Pd1Ni4/CNF) gives only 7% conversion in the reaction of phenylboronic acid and chlorobenzaldehyde after 5 hours at 80 °C using 5 mg of the catalyst (Table 4, entry 1).52 Its performance is insignificant in comparison to that of palladium telluride alloys in the present study. Pd3Te2 is one of those rarest of the rare palladium telluride alloys which have been used to catalyse Suzuki coupling.57 It has been employed to convert bromoarenes into their respective products at 2–3 mol% catalyst loading (Table 4, entry 6).57 Its application in the catalysis of aryl chlorides is not reported. The efficiencies of Pd9Te4 and PdTe nanostructures are also better than those of some nanosized binary phases of palladium sulphides (PdS and Pd16S7) in catalyzing coupling reactions of chlorobenzene (Table 4, entry 11, 12).61 The nanosized Pd16S7, which is generated in situ during the course of a Suzuki reaction using the palladacycle of a thioether ligand as a catalyst, has been isolated and tested independently as a catalyst. Such Pd16S7 nanoparticles catalyze the coupling of only aryl bromides (Table 4, entry 13 and 14) and that too at a high loading.62

In the recent past, organosulphur and organoselenium compounds have been used as stabilizers to obtain uniformly dispersed catalytically active nanoparticles of palladium(0) for Suzuki coupling.58–60 On assessing their performance on various parameters (such as reaction time, catalyst loading and % conversions), it becomes clear that these are less efficient58–60 than the present nanocatalytic systems (i.e. Pd9Te4 and PdTe). The Pd(0) nanoparticles (stabilized with bulky organosulphur ligand) catalyze the coupling of chlorobenzene with phenylboronic acid and give much lesser conversion (∼45%) at 100 °C (Table 4, entry 7).58 In another similar study, Pd(0) nanoparticles (stabilized by anthracene based-organosulphur ligand) have been used to catalyse the coupling of 4-chlorobenzaldehyde (not chlorobenzene) with phenylboronic acid59 and only 75% conversion (Table 4, entry 8) was noticed. It is lower than that observed with Pd9Te4 and PdTe nanocatalysts. However, when anthracene-based organoselenium ligand is used as a stabilizer, similar Pd(0) nanoparticles give better conversions (Table 4, entry 9)59 which is equivalent to those obtained in the present study. Pd(0) nanoparticles, stabilized by didocosyl selenide (i.e. C22H45–Se–C22H45) also show significantly lower efficiency and give only 32% conversion in the catalysis of coupling of 4-chlorobenzaldehyde (Table 4, entry 10).60

Hence, it is inferred that the present palladium telluride alloys have appreciably significant catalytic potential for catalysis of Suzuki coupling of aryl chlorides, the most difficult and unreactive substrates among aryl halides, and also have an edge over the many of the reported catalytic systems either in terms of reaction time, the % conversion or recyclability.

The catalytic potential of nanoparticles of both Pd9Te4 and PdTe has also been investigated for the reduction of nitroarenes. For exploring the possibility of catalytic use in water, 4-nitrophenol (a listed carcinogen pollutant) was chosen as substrate. Both the nanostructures catalyzed the reaction completely within 5.5 minutes. The kinetic studies for 4-nitrophenol reduction (Scheme 1) using PdTe nanostructures (NPs 2) have been carried out using UV-Vis spectroscopy. It was observed that a bathochromic shift appeared in the spectrum when NaBH4 was added because of the formation of the phenolate ion and absorption frequency (λmax) shifts to 400 nm.

The absorption at λmax = 400 nm decreased with respect to time and two new bands appeared at 226 nm and 300 nm respectively [Fig. 11(a)] because of the formation of 4-aminophenol. The reaction was monitored until the band at 400 nm completely disappeared. The rate constant for the reaction has also been determined by plotting a graph of ln[thin space (1/6-em)]Ct/C0 vs. time [Fig. 11(b)]. In this graph, there are two portions labelled ab and bc. Portion ab has very little slope and represents the induction time or the delay in the start of the reaction.


image file: d0ra08732g-f11.tif
Fig. 11 (a) Reduction of 4-nitrophenol (b) plot of ln(Ct/C0) versus time: determination of rate constant.

It occurs when the substrate takes some time to adsorb on the catalytic surface.30 The portion bc has higher slope values and gives the rate constant ‘K’ for the reaction. In the present work, the novel palladium-based catalyst shows high rate constant of 0.265 min−1.

For this reduction reaction too, the present alloy nanostructures are more efficient than many of the known palladium based nanocatalysts (Table 5, entry 1, 4, 5)65,68,69 in terms of rate constant. However, some heterogeneous palladium-based catalysts (immobilized on the solid support) are known to show a better rate constant (Table 5, entry 2, 3).66,67

Table 5 Performance of known palladium based nanocatalytic systems for reduction of 4-nitrophenol in aqueous solution at room temperature
Entry no. Catalyst Time (min) Rate constant (min−1) Ref.
[1] Pd-FG 12 0.141 65
[2] Fe3O4@TA/Pd NPs 4 1.1 66
[3] Pd(II) complex on GO-MnFe2O4 4 0.72 67
[4] Pd-CS/PEO/IA catalyst 30 0.114 68
[5] Au/Ag/Pd trimetallic NPs 20 0.0466 69
[6] Pd9Te4 5.5 0.265 Present study
[7] PdTe 5.5 0.265 Present study


Recyclability of nano-catalysts

The recyclability studies have also been carried out using Pd9Te4 nanostructures for Suzuki Miyaura C–C coupling reaction between 4-chlorobenzaldehyde and phenylboronic acid at 100 °C in aqueous DMF in the presence of Pd9Te4 (NPs 1) as catalyst. The alloy nanoparticles have been found to be recyclable upto six reaction cycles with some loss in the catalytic activity. The nanocatalysts show a slight decrease after every reaction cycle. Conversion is 88% in the first cycle, 87% in second cycle, 80% in the third cycle, 78% in fourth cycle, 75% in fifth cycle and 68% in the sixth cycle. A decrease of around 20% in the conversion of the substrate into the coupled product is observed in the sixth catalytic reaction cycle (conversion = 68%) in comparison to the first reaction cycle (conversion = 88%) (Fig. 12). Hence, it implies that the present alloy nanoparticles are recyclable and can be employed repeatedly in many reaction cycles. Therefore, this alloy may increase the economy of the catalytic process if used as a catalyst.
image file: d0ra08732g-f12.tif
Fig. 12 Recyclability plot of catalytic use of Pd9Te4 alloy nanoparticles in the Suzuki coupling of 4-chlorobenzaldehyde and phenylboronic acid.

Experimental section

Physical measurements

1H, 13C{1H} NMR was carried out on 300 MHz Bruker Spectrospin DPX-300 NMR spectrophotometer at 300.13 and 75.47 MHz respectively. 125Te{1H} NMR was performed on Bruker Advance III 500 MHz Spectrometer at SAIF, IIT Madras. Single crystal X-ray diffraction studies were performed on Supernova X-ray diffractometer system at 150 K using Mo Kα radiation (0.710 Å). CrysalisPro Software (online version) was used for data collection. The structure was solved by direct methods using olex2, SHELXS-97 and refined by full matrix least-squares with SHELXL-97, refining on F2. The image was created using the program diamond. High resolution mass spectrometry (HRMS) was carried out Bruker High Impact HD spectrometer by taking the sample in acetonitrile. Powder X-ray diffraction (PXRD) studies were carried out on Panalytical X'Pert diffractometer with Cu filtered radiation using a scan speed of 2° per min and scan step of 0.02°. The elemental composition of NPs was analysed by using an Energy Dispersive X-ray (EDX) system (Model: JSM 6100). High Resolution Transmission Electron Microscopic (HRTEM) studies were carried out with a FEI Tecnai G2-S-twin electron microscope operated at 200 kV. The specimens for HRTEM were prepared by dispersing the nanoparticles in methanol and ultrasonicating them. Then, the slurry was dropped onto a porous carbon film supported on a copper grid and dried in air. Pervac spectrophotometer was utilized for recording X-ray photoelectron spectroscopy (XPS) data. Dynamic Light Scattering (DLS) studies have been carried out using Malvern zetasizer nano ZSP instrument. Surface area has been analysed on autosorb IQ quantachrome instrument. The N2 adsorption–desorption analysis was carried out using Bruanauer–Emmet–Teller (BET) and Barrett–Joyner–Halenda (BJH) models to get a clear picture of surface area and porosity of the nanomaterials. FTIR has been performed on Shimadzu IRSpirit spectrophotometer.

Chemicals

Diphenyl ditelluride, 2′-hydroxyacetophenone and palladium chloride are procured from Sigma Aldrich. Solvents and other chemicals have been procured from local dealers and were used as received. L1 were prepared according to the reported procedure.70

Synthesis of L2

A solution of L1 (0.25 g, 1.0 mmol) in ethanol was taken in an oven dried round bottom flask and stirred at room temperature. 2'-Hydroxyacetophenone (0.136 g, 1.0 mmol) was added dropwise to the reaction mixture and it was further stirred for 6 hours at room temperature under ambient conditions. The solvent was evaporated and the L2 was dissolved in chloroform and precipitated by the addition of hexane to obtain yellow coloured solid.
L2. NMR: 1H (CDCl3, TMS, 25 °C) δ(ppm): 15.91 (1H, s), 7.77 (2H, d, J = 7.5 Hz), 7.50 (1H, d, J = 8.0 Hz), 7.27–7.31 (2H, m), 7.21 (2H, t, J = 7.5.0 Hz), 6.94 (1H, d, J = 8.5 Hz), 6.78 (1H, t, J = 8.0 Hz), 3.94 (2H, t, J = 7.0 Hz), 3.20 (2H, t, J = 7.5 Hz), 2.26 (3H, s). 13C{1H} (CDCl3, TMS, 25 °C) δ(ppm): 171.82, 163.48, 138.83, 137.56, 132.39, 129.32, 128.07, 127.95, 119.34, 118.73, 117.25, 110.93, 51.13, 14.48, 8.77. 125Te {1H} (CDCl3, Me2Te2, 25 °C) δ (ppm): 467.73.

Synthesis of 1/2

A mixture of L1/L2 (0.1 mmol) and Pd(CH3CN)2Cl2 (0.026 g, 0.1 mmol) was taken in chloroform and stirred at room temperature for 15 minutes at room temperature. The Pd(II) complex was precipitated with the addition of hexane, filtered and dried.
1. Yield (0.0367, 86%), NMR: 1H (CDCl3, TMS, 25 °C) δ (ppm): 8.05 (2H, d, J = 6.0 Hz), 7.37 (2H, m), 7.19 (1H, m), 1.94 (2H, t, J = 7.0 Hz), 1.16 (2H, t, J = 12.0 Hz). 125Te{1H} (CDCl3, Me2Te2, 25 °C) δ(ppm): 1470.69. HRMS (CH3CN): [M − Cl]+ m/z calcd for [C8H11ClNPdTe]+ 391.8777; found 391.8766 (Δ = 2.8%).
2. Yield (0.0437, 80%), NMR: 1H (CDCl3, TMS, 25 °C) δ(ppm): 12.09 (1H, s), 7.98 (2H, t, J = 6.0 Hz), 7.60 (1H, m), 7.32–7.35 (3H, m), 7.23–7.25 (1H, m), 6.73–6.81 (2H, m), 2.40 (3H, s), 2.33 (4H, m). 125Te{1H} (CDCl3, Me2Te2, 25 °C) δ(ppm): 1331.70. HRMS (CH3CN): [M + Na]+ m/z calcd for [C16H16ClNOPdTeNa]+ 531.9017; found 531.9004 (Δ = 2.4%).

Procedure for the development of Pd9Te4 and PdTe nanostructures from Pd(II) complexes 1 and 2

An oven dried three necked flask was purged with nitrogen before the addition of the reactants. 0.5 mmol (0.213 g/0.253 g) of the Pd(II) complex (1/2) was added alongwith 10 mL of oleic acid–oleyl amine solution (5 mL/5 mL). The mixture was heated to 260 °C in case of 1 and 240 °C in case of 2 under N2 with continuous stirring for 2 hours. The colour of the complexes changed from yellow/orange to dark brown within the first 30 minutes and the black precipitate started to form eventually. Thereafter, mixture was cooled to room temperature and acetone (20 mL) was added to isolate the black precipitate which was further separated by centrifugation. The isolated precipitate was washed several times with methanol (20 mL) and dried in vacuo.

Procedure for Suzuki Miyaura coupling reaction of chloroarenes

An oven dried round bottom flask was discharged with chloroarene (1.0 mmol), phenyl boronic acid (1.1 mmol), K2CO3 (2.0 mmol), catalyst (5.0 mg) in aqueous DMF (DMF[thin space (1/6-em)]:[thin space (1/6-em)]Water = 4[thin space (1/6-em)]:[thin space (1/6-em)]1). The reaction mixture was refluxed for 12 hours at 100 °C. After the requisite time, the reaction was cooled and quenched with water. The product was extracted with diethyl ether and dried over anhydrous sodium sulphate. The solvent was evaporated on rotary evaporator. The yield of the product was estimated using 1H NMR spectroscopy.

Procedure for catalytic reduction of nitroarenes

The kinetic studies ascertained to the reduction of 4-nitrophenol have been carried out in quartz cuvettes of path length 1 cm and utilizing a total aqueous volume of 1.0 mL. For each test, a known volume of the catalyst i.e. 10 μL was pipetted out from a stock solution (1.0 mg NPs of 1/2 dispersed in 1.0 mL) in cuvette. To this, 1.0 mL of 10−4 M aqueous solution of 4-nitrophenol was added. Just before the placement of the cuvette in the spectrophotometer, NaBH4 was added. The addition of NaBH4 intensified the colour leading to a bathochromic shift. The absorption spectrum was recorded in the range of 200–800 nm.

Catalytic recyclability

An oven-dried round bottom flask was charged with 4-chlorobenzaldehyde (1.0 mmol, 0.140 g), phenylboronic acid (1.1 mmol, 0.133 g), K2CO3 (2.0 mmol, 0.276 g) and aqueous DMF (DMF[thin space (1/6-em)]:[thin space (1/6-em)]Water = 4[thin space (1/6-em)]:[thin space (1/6-em)]1). Nanoparticles (5 mg of NPs 1), were added to the reaction mixture and the temperature was maintained at 100 °C. The progress of the reaction was monitored with TLC. After completion of the reaction, water and ethyl acetate were added and the mixture was centrifuged. The black residue (i.e. nanocatalysts) was collected and washed with methanol in order to remove the organic content and base. The nanocatalysts were dried in vacuo. The organic layer from water–ethyl acetate was separated and the solvent was evaporated off. The residue was subjected to 1H NMR for conversion estimation. The NPs separated were reused for the next cycle and this procedure was repeated for six times.

Conclusions

The present work involves first study not only on the precursor-architecture controlled synthesis of intermetallic binary phase PdTe and Pd9Te4 nanostructures via single source precursor route but also on their catalytic potential for Suzuki coupling and reduction of nitrophenol. The Pd(II) complexes 1 and 2 of different organotellurium ligands have a major structural difference in terms of coordination mode of the ligand i.e. bidentate in case of 1 and tridentate in case of 2. They function as designers SSPs while undergoing thermolysis under similar conditions and lead to the formation of nanoparticles of different bimetallic alloy materials (Pd9Te4 in case of 1 and PdTe in case of 2). Molecular precursor's architecture controls the composition of the product i.e. nanomaterial. Both the nanostructures do not agglomerate and show uniformity in dispersion. These appear to be spherical in shape. Catalytic studies reveal that nanostructures of both the alloys have catalytic potential for Suzuki–Miyaura C–C coupling of aryl chlorides (the most difficult and unreactive substrates) and reduction of 4-nitrophenol. The nanocatalysts are also reusable upto six reaction cycles, explored in case of Suzuki coupling. The results of this report open a field for development of nanostructures of several binary phases of palladium telluride using easy methods involving single source precursor route. In addition, applications of such nanosized binary phase of Pd–Te alloys will be open for exploration in various fields including catalysis, electrocatalysis, oxygen reduction reactions for use in magnesium air batteries, development of electrodes, etc.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

AA and AK would like to acknowledge Department of Science and Technology, Science and Engineering Research Board (DST SERB) [Project: ECR/2016/001549] for fellowship and financial assistance. Financial assistance provided by UGC under its UGC-BSR Research Start-Up-Grant [No. F.30-371/2017/(BSR) Dated 10 July 2017] is also acknowledged. PO also acknowledges DST for INSPIRE Fellowship [No. DST/INSPIRE Fellowship/2017/IF170491]. SK thanks DST for INSPIRE Faculty Award [DST/INSPIRE/04/2015/002971]. Authors acknowledge SAIF Facility, I.I.T. Madras for 125Te NMR.

Notes and references

  1. L. Polavarapu, S. Mourdikoudis, I. P. Santos and J. P. Juste, CrystEngComm, 2015, 17, 3727 RSC.
  2. D. Jamwal and S. K. Mehta, ChemistrySelect, 2019, 4, 1943 CrossRef CAS.
  3. J. Zhitong, M. Zhang, M. Wang, C. Feng and Z.-S. Wang, Acc. Chem. Res., 2017, 50, 895 CrossRef.
  4. J. D. Major, R. E. Treharne, L. J. Phillips and K. Durose, Nature, 2014, 511, 334 CrossRef CAS.
  5. Q. Huang, F. Dang, H. Zhu, L. Zhao, B. He, Y. Wang, J. Wang and X. J. Mai, J. Power Sources, 2020, 451, 227738 CrossRef CAS.
  6. V. K. Jain and G. Kedarnath, Phys. Sci. Rev., 2018, 4, 20170127 Search PubMed.
  7. M. D. Khan, M. A. Malik and N. Revaprasadu, Coord. Chem. Rev., 2019, 388, 24 CrossRef CAS.
  8. V. K. Jain and R. S. Chauhan, Coord. Chem. Rev., 2016, 306, 270 CrossRef CAS.
  9. R. Zhao, D. Tang, L. Huan, Q. Wu, W. Li, X. Zhang, M. Chen and G. Diao, Sol. Energy, 2019, 178, 241 CrossRef CAS.
  10. S. Kukunuri, S. N. Karthick and S. Sampath, J. Mater. Chem. A, 2015, 3, 17144 RSC.
  11. S. Kukunuri, K. Naik and S. Sampath, J. Mater. Chem. A, 2017, 5, 4660 RSC.
  12. S. Bag, I. U. Arachchige and M. G. Kanatzidis, J. Mater. Chem., 2008, 18, 3628 RSC.
  13. S. C. Sarma, V. Vemuri, V. Mishra and S. C. Peter, J. Mater. Chem. A, 2019, 7, 979 RSC.
  14. S. Kukunuri, M. P. Austeria and S. Sampath, Chem. Commun., 2016, 52, 206 RSC.
  15. S. Gupta, N. Chandna, P. Dubey, A. K. Singh and N. Jain, Chem. Commun., 2018, 54, 7511 RSC.
  16. H. Joshi, K. N. Sharma, A. K. Sharma, O. Prakash and A. K. Singh, Chem. Commun., 2013, 49, 7483 RSC.
  17. K. N. Sharma, H. Joshi, V. V. Singh, P. Singh and A. K. Singh, Dalton Trans., 2013, 42, 3908 RSC.
  18. L. Jiao, F. Li, X. Li, R. Ren, J. Li, X. Jhou, J. Jin and R. Li, Nanoscale, 2015, 7, 18441 RSC.
  19. T. Komatsu, K. Inaba, T. Uezono, A. Onda and T. Yashima, Appl. Catal., A, 2003, 251, 315 CrossRef CAS.
  20. M. Huang, F. Wang, L. Li and Y. Guo, J. Power Sources, 2008, 178, 48 CrossRef CAS.
  21. J. Akhtar, R. F. Mehmood, M. A. Malik, N. Iqbal, P. O'Brien and J. Raftery, Chem. Commun., 2011, 47, 1899 RSC.
  22. S. Dey and V. K. Jain, Platinum Met. Rev., 2004, 48, 16 CAS.
  23. H. Takahashi, N. Konishi, H. Ohno, K. Takahashi, Y. Koike, K. Asakura and A. Muramatsu, Appl. Catal., A, 2011, 392, 80 CrossRef CAS.
  24. K. Mariappan, S. J. P. Varapragasam, M. R. Hansen, S. Rasalingam, M. Alaparthi and A. G. Sykes, J. Organomet. Chem., 2018, 866, 251 CrossRef CAS.
  25. P. Matkovic and K. Schubert, J. Less-Common Met., 1978, 58, 39 CrossRef.
  26. W. S. Kim and G. Y. Chao, J. Less-Common Met., 1990, 162, 61 CrossRef CAS.
  27. D. Kumar, H. Singh, S. Jouen, B. Hannoyer and S. Banerjee, RSC Adv., 2015, 5, 7138 RSC.
  28. J. Yang, X. Wang, Y. Qu, X. Wang, H. Huo, Q. Fan, J. Wang, L. -M. Yang and Y. Wu, Adv. Energy Mater., 2020, 10, 2001709 CrossRef CAS.
  29. J.-H. Liu, L.-M. Yang and E. Ganz, ACS Sustainable Chem. Eng., 2018, 6, 15494 CrossRef CAS.
  30. J.-H. Liu, L.-M. Yang and E. Ganz, J. Mater. Chem. A, 2019, 7, 3805 RSC.
  31. J. J.-H. Liu, L.-M. Yang and E. Ganz, J. Mater. Chem. A, 2019, 7, 11944 RSC.
  32. I. P. Belestkaya, F. Alonso and V. Tyurin, Coord. Chem. Rev., 2019, 385, 137 CrossRef.
  33. M. Orlandi, D. Brenna, R. Harms, S. Jost and M. Benaglia, Org. Process Res. Dev., 2018, 22, 430 CrossRef CAS.
  34. A. Arora, P. Oswal, G. K. Rao, J. Kaushal, S. Kumar, A. K. Singh and A. Kumar, ChemistrySelect, 2019, 4, 10765 CrossRef CAS.
  35. A. Kumar, M. Agarwal and A. K. Singh, J. Organomet. Chem., 2008, 69, 3533 CrossRef.
  36. A. Kumar, M. Agarwal, A. K. Singh and R. J. Butcher, Inorg. Chim. Acta, 2009, 362, 3208 CrossRef CAS.
  37. N. S. Labidi and A. Iddoku, J. Saudi Chem. Soc., 2007, 11, 221 CAS.
  38. F. Lan, J. Bai and H. Wang, RSC Adv., 2018, 8, 16866 RSC.
  39. K. Anand, C. Tikole, A. Phulukdaree, B. Ranjan, A. Chuturgoon, S. Singh and R. M. Gengen, Photochem. Photobiol., 2016, 165, 87 CrossRef CAS.
  40. K. Scheurell, J. Noack, R. Konig, J. Hegmann, R. Jahn, Th. Hofmann, P. Lobmann, B. Litner, P. Gracia-Jaun, J. Eicher and E. Kemnitz, Dalton Trans., 2015, 44, 19501 RSC.
  41. J. Lim, S. P. Yeap, H. X. Che and S. C. Low, Nanoscale Res. Lett., 2013, 8, 281 CrossRef.
  42. A. V. Neimark, K. S. W. Sing and M. Thommes, Handbook of Heterogeneous Catalysis, Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, 2nd edn, 2008, p. 721 Search PubMed.
  43. A. Dhankhar, R. K. Rai, D. Tyagi, X. Yao and S. K. Singh, ChemistrySelect, 2016, 1, 3223 CrossRef CAS.
  44. N. Ghanbari, S. J. Hoseini and M. Bahrami, Ultrason. Sonochem., 2017, 39, 467 CrossRef CAS.
  45. P. Phukan, P. R. Boruah, P. S. Gehlot, A. Kumar, A. Bordoloi and D. Sarma, ChemistrySelect, 2017, 2, 11795 CrossRef CAS.
  46. R. K. Rai, K. Gupta, S. Behrens, J. Li, Q. Xu and S. K. Singh, ChemCatChem, 2015, 7, 1806 CrossRef CAS.
  47. R. K. Rai, K. Gupta, D. Tyagi, A. Mahata, S. Behrens, X. Yang, Q. Xu, B. Pathaka and S. K. Singh, Catal. Sci. Technol., 2016, 6, 5567 RSC.
  48. T.-N. Ye, Y. Lu, Z. Xiao, J. Li, T. Nakao, H. Abe, Y. Niwa, M. Kitano, T. Tada and H. Hosono, Nat. Commun., 2019, 10, 1 CrossRef.
  49. V. Babel and B. L. Hiran, Catal. Lett., 2020, 150, 1865 CrossRef CAS.
  50. D. R. Pye and N. P. Mankad, Chem. Sci., 2017, 8, 1705 RSC.
  51. A. Kumar, G. K. Rao, F. Saleem and A. K. Singh, Dalton Trans., 2012, 41, 11949 RSC.
  52. G. Bao, J. Bai and C. Li, Org. Chem. Front., 2019, 6, 352 RSC.
  53. M. Hajighorbani and M. Hekmati, RSC Adv., 2016, 6, 88916 RSC.
  54. H. Veisi, M. Ghadermazi and A. Naderi, Appl. Organomet. Chem., 2016, 30, 341 CrossRef CAS.
  55. H. Veisi, A. Nikseresht, N. Ahmadi, K. Khosravi and F. Saeidifar, Polyhedron, 2019, 162, 240 CrossRef CAS.
  56. D. Sahu and P. Das, RSC Adv., 2015, 5, 3512 RSC.
  57. G. K. Rao, A. Kumar, M. P. Singh and A. K. Singh, J. Organomet. Chem., 2014, 749, 1 CrossRef CAS.
  58. P. Sharma, A. Arora, P. Oswal, G. K. Rao, J. Kaushal, S. Kumar, S. Kumar, M. P. Singh, A. K. Singh and A. Kumar, Polyhedron, 2019, 171, 120 CrossRef CAS.
  59. P. Oswal, A. Arora, J. Kaushal, G. K. Rao, S. Kumar, A. K. Singh and A. Kumar, RSC Adv., 2019, 9, 22313 RSC.
  60. G. K. Rao, A. Kumar, B. Kumar and A. K. Singh, Dalton Trans., 2012, 41, 4306 RSC.
  61. P. Oswal, A. Arora, S. Singh, G. K. Rao, S. Kumar, A. K. Singh and A. Kumar, Catal. Commun., 2021, 149, 106242 CrossRef CAS.
  62. G. K. Rao, A. Kumar, S. Kumar, U. B. Dupare and A. K. Singh, Organometallics, 2013, 32, 2452 CrossRef CAS.
  63. V. B. Saptal, M. V. Saptal, R. S. Mane, T. Sasaki and B. M. Bhanage, ACS Omega, 2019, 4, 643 CrossRef CAS.
  64. Z. Wang, C. Xu, G. Gao and X. Li, RSC Adv., 2014, 4, 13644 RSC.
  65. G. K. Rao, A. Kumar, J. Ahmed and A. K. Singh, Chem. Commun., 2010, 46, 5954 RSC.
  66. H. Veisi, M. Pirhayati, A. Kakanejadifard, P. Mohammadi, M. R. Abdi, J. Gholami and S. Hemmati, ChemistrySelect, 2018, 3, 1820 CrossRef CAS.
  67. K. Karami and N. S. Mousavi, Dalton Trans., 2018, 47, 4175 RSC.
  68. L. Liang, L. Nie, M. Jiang, F. Bie, L. Shao, C. Qi, X. M. Zhang and X. Liu, New J. Chem., 2018, 42, 11023 RSC.
  69. K. Suwannarat, K. Thongthai, S. Ananta and L. Srisombat, J. Colloid Interface Sci., 2018, 540, 73 CAS.
  70. J. Zakrzewski, B. Huras, A. Kietczewska and M. Krawczyk, RSC Adv., 2016, 6, 98829 RSC.

Footnote

Electronic supplementary information (ESI) available. CCDC 1994615 and 1994616. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/d0ra08732g

This journal is © The Royal Society of Chemistry 2021
Click here to see how this site uses Cookies. View our privacy policy here.