aShenzhen Key Laboratory of Advanced Thin Films and Applications, College of Physics and Optoelectronic engineering, Shenzhen University, Shenzhen, 518060, China. E-mail: yzxie@szu.edu.cn
bCollege of Materials Science and Engineering, Shenzhen University, Shenzhen, 518060, China
cKey Laboratory of Optoelectronic Devices and Systems of Ministry of Education and Guangdong Province, College of Physics and Optoelectronic Engineering, Shenzhen University, Shenzhen 518060, China
First published on 8th April 2021
Fabricating energy-saving, inexpensive and high-activity electrocatalysts for overall water splitting has always been a significant challenge. Electrochemical deposition is considered as a promising method for large-scale industrial applications, but it is prone to generating dense compounds, which reduces the effective catalytic activity area of electrodes. Herein, a low-cost and high-performance bifunctional NiFeMn alloy@NiFeMn oxyhydroxide electrocatalyst was deposited by several minute electrodeposition. Due to the doping of manganese, this method effectively engineers a multi-level dendritic NiFeMn alloy and oxyhydroxide layer, and significantly reduces the energy barrier for the oxygen evolution reaction (OER) and hydrogen evolution reaction (HER), which has been proved by the density functional theory calculations. Specifically, the as-prepared catalyst shows excellent electrocatalytic performance for OER (219 mV) and HER (19 mV) at a current density of 10 mA cm−2. Experimentally and theoretically, the catalyst demonstrated extraordinary performance for overall water splitting and provides a new possibility for industrialization in the future.
Recently, massive efforts have been aimed to research various earth-abundant metal-based electrocatalysts, such as transition-metal chalcogenides, oxides, selenides, borides, nitrides, and phosphides.10–14 Among the abovementioned catalysts, the NiFe-based oxide and oxyhydroxide electrocatalysts have been researched extensively for their high electrolysis performance in alkaline electrolytes.15 Some significant research efforts have been devoted to increase the performance of NiFe-based catalysts, such as special morphology construction, surface defect engineering and integration with some conductive materials.16–18 Specifically, increasing numbers of research studies focus on the construction of active materials by adding new elements to form multi-element catalysts because modulating the energy levels of the catalyst by adding new elements to regulate the electronic structure could change the bond length of the active site and the adsorption energy of the HER/OER reaction intermediates.19 For example, NiVFe trimetallic phosphor nitride was synthesized for overall water splitting, which attained a current density of 10 mA cm−2 with the overpotentials of 79 mV and 229 mV for HER and OER, respectively.20 The two-electrode electrolyzer both fabricated by CoFeZr oxides reached 10 mA cm−2 at 1.63 V for water electrolysis.21 However, there are few studies on multi-element catalysts containing Mn because pure manganese-based oxide catalysts are relatively catalytically inert and exhibit inherent poor conductivity.22 However, manganese plays a crucial role in water oxidation in nature, and it is the third most abundant transition-metal in the earth's crust.23 In order to imitate the green and efficient method of water splitting in nature and reduce the cost of electrocatalyst materials, substantial work still needs to be done for the synergy of Mn and NiFe-based catalysts to increase the bifunctional electrocatalytic activity.
Many breakthroughs have been made in the synthesis of catalysts for the electrolysis of water, but those electrocatalysts are still far away from large-scale water electrolysis. Since many complex chemical or physical methods were used to fabricate the catalysts in order to achieve a better performance than that of the current industrial catalysts, it significantly increases the cost of water splitting.24,25 Additionally, most of the catalysts are in the form of a powder of nanoparticles or nanosheets. A binder will inevitably be used when coating the powders onto the electrode, which will lead to a decrease in conductivity and reduced catalytically active sites.26,27 Although many catalysts are also directly synthesized onto the substrate, their electrochemically active surface area (ECSA) is often subjected to the small surface area of the substrates.28 These factors limit further improvement of the catalyst performance. Meanwhile, the mechanisms among the multiple elements of transition metal catalysts are still not fully mastered. Thus, an in-depth research study on achieving low-cost and high-performance of multi-component catalysts is urgently needed.
Herein, we successfully fabricated NiFeMn alloy (core)–oxyhydroxide nanosheet (shell) arrays (denoted as NiFeMn-AOs) as high-performance bifunctional catalysts for both OER and HER. The NiFeMn-AOs was fabricated on nickel foam (NF) or carbon cloth substrate by chronoamperometry deposition method. The NiFeMn-AOs is cheaper and more environmentally friendly compared with the NiFe-based catalysts synthesized through conventional hydrothermal method or physical vapor deposition method. The particular multi-level dendritic structures of the NiFeMn-AOs samples, which possess larger ECSA and more active sites, facilitate faster electron and ion transfer. As a result, the as-prepared NiFeMn-AOs catalyst shows excellent electrocatalytic performance for OER, attaining a current density of 10 mA cm−2 with a low overpotential of 219 mV and a small Tafel slope of 26 mV dec−1. It also shows excellent stability during a 140-hour test. This catalyst drives a current density of 1 A cm−2 with an ultra-low potential of 1.473 V under harsh industrial conditions. Moreover, it exhibits superior HER performance, and reaches 10 mA cm−2 with an overpotential of only 19 mV in alkaline electrolyte. The result is one of the best records for the NiFe-based catalyst for HER. Furthermore, the two-electrode electrolyzer manufactured by NiFeMn-AOs shows outstanding performances on water splitting, achieving 15 mA cm−2 at a low voltage of 1.46 V. The current density can reach 500 mA cm−2 when the voltage of the electrolytic cell is 2.1 V in 1 M KOH. The fundamental mechanism of Mn doping in the NiFeMn-AOs behind the excellent performance of OER and HER has been studied by density-functional-theory (DFT) calculations. The conclusion drawn from the experimental data and DFT calculation shows that NiFeMn-AOs has both outstanding HER catalytic activity and strong OER activity, which provides a new possibility for industrial application in the future.
The NiFe-AOs and Ni/NF electrodes were prepared as reference electrodes by an essentially identical procedure with adjusting the molar ratio of Mn, Ni and Fe metal ions in electrodeposition solution. The overall molar amount of metal ions in the electroplating bath is the same. The Ni/Fe ratio of NiFe-AOs is 2:1 and the Ni/NF only with Ni2+. The method of manufacturing the flexible NiFeMn-AOs electrode was made in the same way, except that the nickel foam substrate was replaced by a carbon cloth substrate.
ERHE = EAg/AgCl + 0.0591 × pH + EΘAg/AgCl |
Before the test, the electrode was subjected to 20 cycles of 100 mV s−1 scan rate by cyclic voltammetry to activate the electrode material. The OER and HER performances of the electrodes were characterized by linear sweep voltammetry (LSV) at a sweep rate of 1 mV s−1 to avoid the possible contribution of the capacitive current. Electrochemical impedance spectroscopy (EIS) was applied to measure the ohmic resistance of the electrocatalytic system. The test frequency range of EIS was 105 Hz–0.1 Hz, and the amplitude was 5 mV. The electrode potential was corrected with a value of 95% × Rs through the workstation, where Rs is the ohmic resistance obtained by EIS. The ECSA values of the as-prepared electrodes were calculated from the electrochemical double-layer capacitance (Cdl) of the electrode morphology. The Cdl values of the electrodes were calculated on the basis of the cyclic voltammetry curves recorded in a non-Faradaic range at various sweep rates (20, 40, 80, 160, 240, 320 and 400 mV s−1), and it was calculated by difference of the current density plot (Δj) against the sweep rate, where the Cdl is half of the resulting linear slope. The Tafel slope of the polarization curve was calculated by plotting the overpotential and the logarithm of the current density. The long-term stability of the electrocatalyst was evaluated by chronopotentiometry and multi-step chronopotentiometry. The Faraday efficiencies of HER and OER were calculated by comparing the volumes of oxygen and hydrogen that were collected by the replacement water, and the electricity consumed from water splitting.
After the NiFeMn-AOs catalyst was synthesized, the surface topography of the electrode was probed by SEM. The SEM images show that (Fig. 1b) a lot of highly porous coral-like structures with sizes from 1 μm to 5 μm are on the NF substrate. At relatively higher magnification, as shown in Fig. 1c, many ultrathin nanosheet architectures are over the coral-like structure, forming a multi-level catalytic system. This revealed that the NiFeMn oxyhydroxide was homogeneously grown on the NiFeMn alloy skeleton. Compared with NiFe-AOs, this structure provides a high surface area with more reactive sites, and also promotes the release of oxygen or hydrogen bubbles from the catalyst (Fig. S2†). The contact angle test demonstrates that the hydrophilicity of the NiFeMn-AOs electrode is significantly improved compared with the foamed nickel (Fig. S3†). These properties are beneficial to the OER and HER process, and it is more obvious under larger current density. In addition, the elemental mapping of EDX illustrated that the multi-level structure is composed of Ni, Fe, Mn and O elements, and they are homogeneously distributed in the electrode (Fig. 1d). The pictures of TEM and HAADF-STEM in Fig. 1e and Fig. S4,† respectively, illustrate that the NiFeMn-AOs is coated with an ultrathin nanosheet array. As shown in the high-resolution TEM (HRTEM) image (Fig. 1f), the nanosheets consist of both nanocrystal and amorphous parts, and the formed lattice spaces of 0.258 nm are attributed to NiFeMn oxides (311). Moreover, the corresponding diffraction rings pattern was obtained by selected area electron diffraction (SAED). They could be assigned to the (220), (311), (400), (511), and (440) planes of the NiFeMn oxides. The NiFeMn oxyhydroxide exhibits a diffuse halo ring between the circles. The above results confirm that the NiFeMn-AOs with multi-layer structure was deposited onto the surface of the nickel foam by the one-step electrodeposition method.
To further analyze the phase composition and crystallinity of NiFeMn-AOs, the XRD pattern was tested, as shown in Fig. S5.† Only the diffraction peak of the NF substrate is found in the patterns of XRD. This result proves that the major structure of NiFeMn-AOs is amorphous. The amorphous structure is usually associated with more reactive sites. After the samples were annealed in a nitrogen atmosphere at 500 °C for two hours (denoted as t-NiFeMn-AOs and t-NiFe-AOs), except for the peaks indexed to NF, two peaks at 29.8° and 35.2° can be indexed to the (220) and (311) planes, respectively, of the cubic structure of NiFe2O4 (JCPDS no. 74-2081) for the t-NiFe-AOs. Compared with t-NiFe-AOs, the position of the peak of t-NiFeMn-AOs exhibits minor left shifts with the Mn doping, and a new minor peak at 36.7° can be indexed to the (211) plane of MnO2 (JCPDS no. 44-0141).37 These results clearly illustrated the successful formation of the NiFeMn oxyhydroxide overlayers on the NiFeMn alloy, and the incorporation of Mn into the electrode.
Furthermore, XPS was applied to detect the major chemical composition and chemical bonding state of the catalyst surface. Specifically, the XPS survey spectrum of the NiFeMn-AOs indicated the coexistence of nickel, iron, magnesium and oxygen elements on the sample surface (Fig. 2a). The high-resolution spectra of Ni 2p (Fig. 2b) show two main peaks corresponding to Ni 2p3/2 and Ni 2p1/2, and two minor peaks made up of their satellites peaks (Sat.). Peak fitting indicated the co-existence of Ni2+ (855.2, 872.6 eV) and Ni3+ (856.3, 873.9 eV), which can be ascribed to Ni(OH)2 and NiOOH, respectively, while two minor peaks (852.5, 869.9 eV) are allocated to Ni0 (metallic Ni).38,39 In particular, we noticed that the ratio of the Ni3+/Ni2+ peak intensity in NiFeMn-AOs was higher than that of NiFe-AOs. This indicated that there was more NiOOH, which is a key active intermediate with lower OER overpotential.40 Similarly, the deconvoluted peaks of the Fe 2p spectrum (Fig. 2c) revealed Fe2O3 (710.2, 723.7 eV) and FeOOH (713.0, 725.9 eV) in the sample, and two minor peaks (706.6, 720.1 eV) are allocated to Fe0 (metallic Fe). The peak at 711.7 eV can be ascribed to the LMM Auger line of the Ni element, while using Al Kα radiation.13,41 The Fe2O3 on the surface may be generated from Fe(OH)3, which was dehydrated in air and converted to Fe2O3. The binding energy of the Fe 2p peaks in NiFeMn-AOs is more positively shifted, and its peak intensity is lower compared with that of the NiFe-AOs. Moreover, compared with the distinct signals of Ni3+/Ni2+ and Fe3+, the signal of Ni0 or Fe0 is significantly weaker. This phenomenon is due to the deposition of a thin array of amorphous nanosheets on the surface of the electrodes, and it is difficult to detect the photoelectrons generated by the alloy of the skeleton. The high-resolution spectra of Mn 2p are shown in Fig. S6a.† Unfortunately, the peak of Mn 2p3/2 overlaps with the strong LMM Auger line of the Ni element signals, which makes it difficult to get a precise spectral analysis of the Mn 2p.42 However, the minor Mn 3p peak at 48 eV in the full spectra indicates the existence of Mn. As shown in Fig. S6b,† two multiple-splitting peaks exist in the Mn 3s spectrum. The binding energy difference between the peaks is 6.3 eV, which reveals that the major valence state of Mn existing in the electrode is Mn2+.43 The O 1s spectrum exhibited two peaks (529.8, 531.3 eV); they are allocated to metal-O and metal-OH, respectively. Compared with the NiFe-AOs, the NiFeMn-AOs sample shows more metal-OH on the surfaces, which could obviously improve the OER efficiency.44
Fig. 2 (a) Wide-scanning XPS survey of the NiFeMn-AOs. (b–d) XPS high-resolution scans of (b) Ni 2p, (c) Fe 2p and (d) O 1s. |
The electrocatalytic properties of the as-prepared NiFeMn-AOs electrode were directly measured by LSV in a three-electrode cell in 1 M KOH electrolyte. The scanning rate was at 1 mV s−1 in order to avoid metal ion redox overlap with the OER polarization curves. For comparison, bare nickel foam, RuO2/NF, Ni/NF and NiFe-AOs electrodes were also measured. As the OER polarization curves illustrated in Fig. 3a, the state-of-the-art RuO2/NF shows good OER activity. It required overpotentials of 286 mV and 340 mV to attain current densities of 10 mA cm−2 and 200 mA cm−2, respectively. The NF substrate shows hardly any OER activity (370 mV and 493 mV). The NiFeMn-AOs shows the smallest overpotential (219 mV and 268 mV) among all the electrodes we tested. This electrocatalytic activity exceeds the performance of the OER electrocatalysts that have been recently reported (Table S1, ESI†), indicating that the NiFeMn-AOs catalysts could significantly lower the activation energy for the OER reactions. To further evaluate the OER reaction kinetics of these electrocatalysts, the corresponding Tafel analysis was calculated from the LSV curves (Fig. 3b). The Tafel slope value of NiFeMn-AOs is 26 mV dec−1, which is smaller than that of NiFe-AOs (31 mV dec−1), and it is obviously lower than those of Ni/NF (63 mV dec−1), RuO2 (89 mV dec−1) and foamed nickel (86 mV dec−1), indicating the fast OER reaction kinetics of the NiFeMn-AOs catalyst.
To demonstrate the origin of the intrinsic activity of the different catalysts, the ECSA was determined by measurement of different electrodes conducted at double layer capacitance (Cdl). Fig. 3c is based on the cyclic voltammetry curves under different sweep rates, where the current response occurred within the non-Faraday charging potential range of the double layer. The Cdl value of the NiFeMn-AOs sample is 24.2 mF cm−2, which is 4.52 and 11 times larger than the values of the NiFe-AOs and Ni/NF samples, respectively. Generally, the larger Cdl suggests larger ECSA and more exposed active sites, which show that the multi-level nanosheet arrays on NiFeMn-AOs are beneficial to get larger surface areas and higher catalytic activity. In addition, we found that it is easier to generate relatively dense NiFe alloys in the electrochemical deposition process if only nickel and iron metal elements are in the electroplating bath, resulting in a smaller ECSA compared to NiFeMn-AOs under the same deposition condition. This phenomenon was more pronounced when only nickel metal elements are electrodeposited. Moreover, the doping of Mn can significantly increase the conductivity of the metal oxyhydroxide, which means that the effective activity of the catalyst is improved.37,45 From the EIS Nyquist plots in Fig. 3d, the NiFeMn-AOs has a smaller charge-transfer resistance (Rct) (2.72 ohms) compared with RuO2/NF (10.9 ohms) and the NiFe-AOs (3.4 ohms), showing high efficiency in the charge transport and excellent OER dynamics.
The stability of NiFeMn-AOs was also obtained by multi-step chronopotentiometry test in 1 M KOH. As shown in Fig. 3e, the current range is from 10 to 500 mA cm−2 for a total of 140 hours (10, 100, 200, 300, 400, 500 and 10 mA cm−2 per 20 hours) in the experiment. At the beginning of 10 mA cm−2, the initial value of the potential is at 1.466 V. When the test is completed and the current returns to 10 mA cm−2, the cell potential is 1.474 V, with only 8 mV overpotential increasing. This result suggests that the NiFeMn-AOs has outstanding mass transportation, mechanical robustness and durability. Moreover, after consecutive 2500 cycles with a sweep rate of 100 mV s−1 in the range from 1.2 to 1.5 V, the NiFeMn-AOs still performed efficiently with even a slight increase compared with the initial value. This phenomenon may be due to the alloy on the surface being oxidized to form more active sites (Fig. S7†).46
The HER performance of the NiFeMn-AOs catalyst was also measured on a three-electrode cell in 1 M KOH electrolyte. As shown in Fig. 4a, the NiFeMn-AOs reveals outstanding catalytic performance with the ultra-low overpotentials of 19.5 mV and 112.2 mV to attain the current densities of 10 mA cm−2 and 200 mA cm−2, respectively. This result is better than that of NiFe-AOs (70.6 mV, 236.4 mV), Pt plate (38.5 mV, 239.8 mV) and NF (140 mV, 389.5 mV). The catalytic ability of the NiFeMn-AOs sample is also one of the strongest non-noble metal catalysts and bi-functional catalysts to be recently reported (Table S2, ESI†). The NiFeMn-AOs exhibit excellent HER activity compared to NiFe-AOs and Pt plate, indicating that the Mn doping is beneficial to increasing the HER catalytic activity.47 The Tafel slope calculated from the polarization curve are shown in Fig. 4b, the NiFeMn-AOs with a smaller Tafel slope (45 mV dec−1) as compared with Pt plate (69 mV dec−1), the NiFe-AOs (125 mV dec−1) and the pure NF (174 mV dec−1), indicating the NiFeMn-AOs with faster HER reaction kinetics.
In addition, the durability of the electrochemical reaction is also a vital factor in assessing the comprehensive performance of the catalyst. The multi-step chronopotentiometry curve of NiFeMn-AOs with seven constant current densities (10, 100, 200, 300, 400, 500 and 10 mA cm−2 per 600 s) is shown in Fig. 4c. The overpotential of the sample had a negligible increase after the durability test. Moreover, the NiFeMn-AOs shows a slight activity decay after long-term stability over 50 h by chronopotentiometry measurement (Fig. S8†). These results demonstrate that the NiFeMn-AOs have preeminent HER performance and good stability in an alkaline electrolyte. Similarly, from the EIS Nyquist plots in Fig. 4d, the NiFeMn-AOs has much smaller Rct compared with the Pt plate and Ni/NF, with the smallest Rct value of 1.52 ohms. This result demonstrates that there is faster electron transport kinetics for HER between the interface of the electrolyte and NiFeMn-AOs. Combined with the abovementioned results, doping of Mn by electrodeposition is an effective method for increasing the catalytic performance of HER for NiFeMn-AOs in alkaline electrolyte.
To further understand the catalytic mechanism of the NiFeMn-AOs, the sample was annealed at 500 °C for two hours in the nitrogen atmosphere. The OER and HER performance of the electrode significantly decreased after annealing, which could be caused by the decrease in ECSA of the electrode after annealing. Furthermore, a relatively low activity of the metal oxides was formed on the surface of the catalyst due to the dehydration of the metal oxyhydroxide (Fig. S9†). Moreover, the catalytic performance of the NiFeMn-AOs electrode was tested under extreme conditions, such as high temperature and concentrated alkaline solution, which are commonly used in commercial alkaline water electrolysers. Fig. 4e and Fig. S10† reveal the OER and HER polarization curves of NiFeMn-AOs in 6 M KOH at 60 °C, respectively. The NiFeMn-AOs electrode shows outstanding activity under harsh industrial conditions. It delivered a current density of 10 mA cm−2 and 1 A cm−2 at 1.36 V and 1.473 V for OER, respectively. When the cell voltage reached −0.131 V, the current density attained 200 mA cm−2 for HER. These results completely satisfy the requirements for commercial water electrolyser applications.
Raman spectroscopy was applied to research the surface of the NiFeMn-AOs before and after OER or HER (Fig. 5a). Three obvious broad peaks can be measured for the original NiFeMn-AOs. The bands at around 488 and 596 cm−1 are due to the Ni–O stretching vibrations in the disordered Ni(OH)2 clusters. The frequency of the Ni–O stretching vibrations of the NiFeMn-AOs is higher than that of pure Ni(OH)2, which is due to the insertion of Fe and Mn into the lattice of Ni(OH)2.41,48 The Raman bands at 662 cm−1 may be attributed to the amorphous FeOOH on the electrode.49 After the process of OER, the peak of Ni(OH)2 shifts to the left and the peak intensity of FeOOH increases significantly, which corresponds to the production of OER catalytically active substances.50 After HER treatment, most of the oxyhydroxides on NiFeMn-AOs are reduced to metals, so the intensity of the Raman peak is significantly reduced. The minor peak corresponding to Ni(OH)2 appears only at 566 cm−1.51
For further development toward industrialized application, it is essential to research the overall water splitting with synergistic converting water to oxygen at the anode and hydrogen at the cathode. Since NiFeMn-AOs exhibits the superior bifunctional performance for OER and HER, an overall water splitting electrolyzer was manufactured through using the NiFeMn-AOs as the anode and also the cathode electrode in 1.0 M KOH electrolyte. The LSV curve of the overall water electrolysis of different samples is presented in Fig. 5b. The NiFeMn-AOs shows the high performance of water electrolysis with a cell voltage of 1.46 V to provide a current density of 15 mA cm−2. This result is superior to the Pt plate//RuO2 (1.59 V), and the bifunctional electrocatalysts that have been recently reported for overall water splitting (Table S3, ESI†). The long-term stability is a key index of the durability of the water electrolyzer. We tested the overall water splitting durability of the NiFeMn-AOs. The result is shown in Fig. 5c. The multi-step chronopotentiometry curve of NiFeMn-AOs had seven constant current densities for a total of 13 hours, and the overpotential has a negligible increase after the test (with only 5 mV). These results indicate that NiFeMn-AOs is a promising non-noble metal catalyst for practical water electrolysis. Moreover, we also measured the polarization curve of the NiFeMn-AOs//NiFeMn-AOs electrolyzer in 6 M KOH at 60 °C and its corresponding durability at 200 mA cm−2 (Fig. S11†). The NiFeMn-AOs shows high performance of overall water splitting in commercial alkaline water with an ultra-low voltage of 1.41 V at a current density of 10 mA cm−2 and at 1.60 V for 100 mA cm−2, indicating that the NiFeMn-AOs has great potential for industrial application. The faradaic efficiency of this electrolyzer for H2 and O2 generation was also evaluated by water displacement method (Fig. 5d). The proportion of the H2 and O2 volume is close to 2:1. The moles of the collected H2 and O2 are consistent with the result of theoretical calculation by Q = I × t, which showed over 99% faradaic efficiency for the HER and OER processes. Finally, these catalytic results demonstrated that the NiFeMn-AOs have great potential for cosmically commercial applications of hydrogen and oxygen production with low-cost and high performance.
The above experimental measurement results illustrate that with the introduction of Mn into NiFe-AOs, the catalyst could obviously increase the catalytic performance for OER and HER. In order to reveal the essential mechanism of the catalyst performance enhancement (except the increasing of ECSA), DFT was applied to elucidate the OER and HER processes on NiFeMn-AOs. The optimized surface models of NiFeMn-AOs and NiFe-AOs (Fig. S12†) were built on the basis of the NiFe LDH bulk. The calculated adsorbed H* (ΔGH*) values on NiFeMn-AOs and NiFe-AOs are 0.47 and 1.19 eV, respectively (Fig. 6a). The lower value on NiFeMn-AOs elucidates that NiFeMn-AOs is more efficient than NiFe-AOs for the HER process, which is in accordance with the results of the electrochemical experiments. Moreover, the classical four-electron step mechanism was adopted to describe the OER in alkaline electrolyte.52 Thus, the adsorption energy of OH*, O* and OOH* species on NiFeMn-AOs and NiFe-AOs were calculated (Fig. 6b). The formation of OOH* is the rate-determining step (RDS) on NiFe-AOs with the energy barrier of 1.32 eV at U = 1.23 V. However, the RDS becomes the deprotonation of *OH to *O for NiFeMn-AOs with the energy barrier of 0.84 eV, which means that NiFeMn-AOs is more efficient than NiFe-AOs for OER. The above calculations show that the doping of Mn can significantly improve the HER and OER activities of the NiFeMn-AOs catalyst.
Fig. 6 (a) Gibbs free-energy diagram of the HER process of NiFe-AOs and NiFeMn-AOs. (b) Gibbs free-energy diagram of the OER process at 1.23 V for NiFe-AOs and NiFeMn-AOs. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1qi00215e |