Open Access Article
Jwala Patela,
Biswajit Majib,
N. S. Hari Narayana Moorthya and
Sabyasachi Maiti
*a
aDepartment of Pharmacy, Indira Gandhi National Tribal University, Amarkantak, Madhya Pradesh-484887, India. E-mail: sabya245@rediffmail.com; Tel: +91 9474119931
bDepartment of Chemistry, Indira Gandhi National Tribal University, Amarkantak, Madhya Pradesh-484887, India
First published on 21st July 2020
Natural polysaccharides are well known for their biocompatibility, non-toxicity and biodegradability. These properties are also inherent to xanthan gum (XG), a microbial polysaccharide. This biomaterial has been extensively investigated as matrices for tablets, nanoparticles, microparticles, hydrogels, buccal/transdermal patches, tissue engineering scaffolds with different degrees of success. However, the native XG has its own limitations with regards to its susceptibility to microbial contamination, unusable viscosity, poor thermal and mechanical stability, and inadequate water solubility. Chemical modification can circumvent these limitations and tailor the properties of virgin XG to fulfill the unmet needs of drug delivery, tissue engineering, oil drilling and other applications. This review illustrates the process of chemical modification and/crosslinking of XG via etherification, esterification, acetalation, amidation, and oxidation. This review further describes the tailor-made properties of novel XG derivatives and their potential application in diverse fields. The physicomechanical modification and its impact on the properties of XG are also discussed. Overall, the recent developments on XG derivatives are very promising to progress further with polysaccharide research.
![]() | ||
| Fig. 1 Chemical structure of (a) XG (chair conformation); (b) XG (Haworth projection); (c) carboxymethyl XG; (d) carboxymethyl hydroxypropyl XG. | ||
The hydroxy and carboxy polar groups of XG reconnoiter intramolecular and intermolecular hydrogen bonding interactions in aqueous solution.6 Due to high molecular weight and hydrogen bonding interactions, an aqueous solution of XG exhibits high intrinsic viscosity at low concentration,7 and behaves like a pseudoplastic fluid.8 High viscous rheology and pH- and salt-resistant properties of XG are satisfactory for use as thickening agent, suspending agent,9,10 and stabilizers for food, pharmaceuticals, cosmetics11–14 and drag reducer in oil drilling.15 XG assumes disorder conformation under low ionic strength or high temperature;16 however, the XG present themselves either in single or double helix conformations under reverse condition.17 As a consequence of 3-D association of XG chains, its aqueous solution confers weak gel-like properties.18 However, XG never forms true gels at any concentration,19 attributable to its weak, non-covalent intermolecular interactions. In comparison to gels, hydrogels are crosslinked 3-D networks of hydrophilic polymers which swell in water or biological fluids but do not dissolve. Hydrogels possess some other interesting characteristics such as biocompatibility, softness which put them forward as carriers for drug or proteins delivery.20 Cross-linking of XG can be done either by physical or chemical methods.21,22 Physical cross-linking is a well-established method to fabricate XG-based hydrogels.23 In this method, the concentrated polysaccharide is cross-linked through hydrogen bonding,24 electrostatic ionic force,25 π–π stacking,26 hydrophobic interaction, or host–guest inclusion27 to obtain hydrogels. However, the physically-formed hydrogels suffer from poor mechanical strength, perhaps due to intermolecular secondary interactions, generally weaker than covalent bonds.28 Further, the lack of thermal stability, pH or salt stability on aging limits their applications. On heating or dilution, XG physical gels are easily solubilized in aqueous solution29 and thus, they are not suitable as controlled drug release carrier. In contrast, the coordination bonding between XG polymer chains and trivalent metal ions leads to stable gels via dimeric or polymeric ionic bridges.30,31
XG has also been put forward as a component of hydrogel preparations with other polymers such as alginate, locust bean gum, chitosan in the form of microparticles32,33 and nanoparticles.34,35 One fascinating example is the combination of XG with locust bean gum. In equal proportion, they can form a firm, thermoreversible gel in aqueous medium through synergistic interaction.36 This observation captivates this polymer combination for use as control drug release carriers.37
It is noteworthy that XG can act as a stabilizer for the synthesis of gold nanoparticles. The presence of mannose sugars in XG further assist in the delivery of chemotherapeutic agents/siRNA/shRNA to mannose receptor overexpressing cancer cells.35 Nonetheless, XG-stabilized silver nanoparticles have been studied for their antibacterial and catalytic applications.38 As a coating material, XG appears promising for the production of iron nanoparticles of 20–80 nm diameters.39 Recently, liposomes coated with chitosan–XG have been proposed as potential carriers for direct drug administration to lungs due to their improved liposomal stability and mucoadhesion properties.40,41
Native XG has been extensively studied as matrix forming materials in the design of tablets either alone42–47 or in combination with other natural polymers such as guar gum,48 alginate,49,50 cashew gum,51 konjac glucomannan,52 Gleditsia sinensis Lam. galactomannan,53 Mimosa scabrella galactomannan54 for the controlled delivery of various kinds of drugs. Chitosan and XG is an entrancing binary composition. The anionic gum electrostatically interacts with chitosan and forms polyelectrolyte complexes which serve as release-retardant for drugs.55,56 Even, the biocompatibility of chitosan–xanthan polyionic complex favors its pharmaceutical application.57
XG is not digested in human stomach or small intestine, but degraded in presence of colon enzymes.58 Thus, XG matrices can shield the drug from the environments of stomach and small intestine and deliver the drug to the colon. On reaching colon, they are assimilated by the anaerobic microflora of the colon, for example, bacteroides, bifidobacteria species and eubacteria, to smaller monosaccharides, which are then either used as energy source by the bacteria or degraded by enzyme. Keeping this in view, XG-based colon drug delivery systems are devised and tested for possible colon targeting of drugs. The systems are not limited to XG59 but include other polymers such as konjac glucomannan,60 chitosan/eudragit,61 guar gum62 as a component.
XG has an excellent biomimicking potential for tissue engineering applications such as bone, cartilage, and skin regeneration. XG-based hydrogels composed of other natural polymers and nanohydroxyapatite are fabricated and tested for tissue engineering applications63,64 and cellular uptake studies.65 In addition, the use of XG with electroactive polypyrrole has shown significant improvement in fibroblast proliferation.66 Kumar et al.67 found that XG-based hybrid scaffold system supported cell adhesion and proliferation of preosteoblast cells and thus seemed suitable for tissue engineering applications.
Its topical drug delivery application via intranasal, ocular, buccal and transdermal routes is also noteworthy. With large surface area, porous endothelial membrane and high total blood flow bypassing hepatic, gut wall metabolism and/or destruction in the gastrointestinal tract,68 the intranasal route appears to be a reliable alternative to oral and parenteral route for drug delivery. For example, XG-based in situ nasal gel has shown its unique ability to enhance drug permeation, bioavailability, and deliver drug directly to brain via olfactory lobe pathway.69–72 In context of ocular therapy, the major problem lies in attaining optimal drug concentration at the site of action. This is largely due to precorneal loss as a consequence of blinking of eyes.73 In situ gel forming system appears to be the solution to this problem. The ocular bioavailability can be enhanced by increasing pre-corneal retention time. Accordingly, in situ ocular gels of XG in combination with other polymers such as poloxamer-407–guar gum,74 HPMC K4M,75 alginate–carbopol 934,76 gellan gum,77,78 alginate–ethylcellulose,79 poloxamer 407/188 (ref. 80) have been tested. Ion-induced nanoemulsion-based in situ gelling system of XG with HPMC or carbopol is also examined.81 Reports on in situ vaginal gels for eradication of candidiasis82 and in situ gel forming tablets83 are also evident. XG-based ophthalmic liquids,84 vaginal gels,82,85 bioadhesive liquids laden with lipid nanoparticles,86 microemulsion-based hydrogel87 and additives for spray-drying and freeze-drying processes88,89 are reported as well.
There is an expanse of smooth muscle and immobile mucosa in buccal cavity, which sets a platform for delivering drugs directly to the systemic circulation through the internal jugular vein, thus avoiding hepatic metabolism and acid hydrolysis in the gastrointestinal tract.90 Moreover, rapid mucosal cell recovery is attractive for opting buccal route for drug delivery purpose.91 These inspired researchers to develop nicotine patches for smoking cessation,92 desloratidine patches for treating allergic rhinitis93 and zolmitriptan patches for migraine treatment.94 Transdermal patches further provide benefits in terms of reduced first-pass metabolism, frequency of dosing, side effects secondary to gastrointestinal intolerance and fluctuations in drug levels.95 Transdermal films/patches of XG with other polymers such as alginate,96,97 hydroxypropylmethyl cellulose–carboxymethyl cellulose98 are reported for analgesic and antihypertensive drugs.
The beneficial effects after oral administration of XG on immune-surveillance against neoplasms are also reported.99 Low-molecular-weight XG (4.07 × 104 Da) has shown antioxidant and excellent protective effect on H2O2-injured Caco-2 cells, suggesting its use in food/pharmaceuticals in order to alleviate/resist oxidative damage induced by overproduction of reactive oxygen species.100 XG is a strong inhibitor of oil peroxidation101 and antioxidant for human corneal epithelial cells at 0.2% strength.102
Despite numerous potential benefits, native XG poses some problems which include microbial contamination, unstable viscosity, poor shear resistance, inadequate mechanical, thermal properties and uncontrolled rate of hydration. These limit its applications in food, pharmaceutical and biomedical fields. Further, XG dissolves at a slow rate particularly in cold water at high concentration. Upon dispersion, it forms lumps in water called fish eyes103 due to its improper hydration. Consequently, a gelatinous outer layer is formed on surface of the particles, immediately after dispersion. This gelatinous layer prohibits water penetration and hinders complete dissolution of the particles.104 Due to insufficient gelling, XG itself fails to afford self-sustainable, stable hydrogel beads in presence of metal ions. XG possesses a number of hydroxy and carboxy groups which are amenable for chemical modification with successive improvement in its physicochemical properties especially solubility, swelling and metal-induced gelling ability; mechanical and thermal stability. The chemical derivatives then become widely acceptable for diverse applications. As extracted from scientific literatures, the chemical modification of XG involves etherification, esterification, acetalation, oxidation, peptide linking, ionic and covalent crosslinking, and mechanical modification. However, there are no decent reviews that sum up the data on modification procedures of XG, resultant properties and the diverse application of XG derivatives.
Though some reviews cover industrial production,105–107 and drug delivery and biomedical applications of XG,108–111 these are not adequate. In 2003, Badwaik et al.112 published a review on XG and its derivatives which discussed the synthesis of acetalated and carboxymethyl derivatives of XG, microwave and plasma assisted grafting of XG. The authors mostly focused on drug delivery application. However, this review lacks significant, in-depth and detailed up-to-date information on synthetic procedures, properties and diverse applications of modified xanthan polysaccharide. Till date, no review article describes XG derivatives in a comprehensive manner in terms of their detailed synthetic/crosslinking procedures, tailored properties beneficial for industrial applications in the field of pharmaceutical and biomedical science and technology. This review attempts to cover these aspects of XG derivatives to fulfill the unmet needs of students, researchers, and budding scientists in these fields.
:
XG ratio within 0.5 to 3.113 The viscosity, elastic modulus and molecular weight of XG are lessened after modification. The derivative becomes more hydrophilic than native XG with gradual increase in degree of substitution. However, the shear-thinning and weak gel behaviors of XG are not affected after carboxymethylation. In contrast, an aqueous solution of carboxymethyl hydroxypropyl XG (Fig. 1d) exhibits greater viscosity, elastic modulus, and temperature- and shear-resistance than XG solution at the same strength. A better proppant carrying ability makes this derivative suitable for use as an additive of fracturing fluids.114
Similar viscoelastic behaviors are noticed for cationic and amphoteric XG derivatives, synthesized using N-(3-chloro-2-hydroxypropyl)trimethyl ammonium chloride115,116 and 3-chloro-2-hydroxypropyldimethylhexadecylammonium acetate,117 respectively. The amphoteric XG solution appears to be a better drag reducer than virgin XG solution. Oleamidopropyl dimethylamine- and triisopropanolamine-modified amphoteric derivatives of xanthan have been reported for their high viscosity (Fig. 2).118
The etherified derivatives of XG have been assessed for their quality attributes in the form of hydrogel films. Alupei et al.119 synthesized epichlorohydrin-crosslinked poly (vinyl alcohol) (PVA)/XG supersorbent hydrogel films (1 mm thickness) under basic medium and appraised their controlled swelling in vitro. Interestingly, higher polymer
:
crosslinker ratio (5
:
1) allowed swelling of the hydrogels up to ∼2500%. Dhar and collaborators120 highlighted the importance of pH on crosslinking reaction of epichlorohydrin with PVA/XG. They perceived that labile ester linkages predominated in the composite films at pH < 4; whereas both ether and ester bonds were registered over pH 7.0–7.5 and consequently, manifested different degrees of swelling in water. They argued that the films synthesized at pH > 9 were mechanically strong due to ether linkages and thus swelled progressively. Incorporation of XG in PVA films caused lesser swelling of the composite films and proved useful in controlling release of uric acid over 24 h at pH 7.4 (Fig. 3).
Zhang et al.121 spotted highly viscous, thixotropic, viscoelastic and thermoresistant characteristics of XG after crosslinking under alkaline condition at epichlorohydrin
:
XG weight ratio of 4
:
200, beyond which these additive effects nullified. The crosslinking effect of epichlorohydrin on theophylline loading and release from xanthan/chondroitin sulfate (1
:
1) hydrogels was assessed by Oprea et al.122 They noted that about 78% theophyline loading was possible by diffusion filling method. The hydrogels swelled within a minute but thereafter absorbed simulated gastric and intestinal fluids at a slower rate. The inclusion of chondroitin sulfate in the hydrogels suppressed drug release by 34% in acidic fluid (pH 2.2) in 7 h. However, they spotted a reverse phenomenon in intestinal fluid (pH 7.4). An enhanced oral bioavailability of 323% clearly provided an indication of preclinical success of this hydrogel system.
Maiti and groups123 proposed hexadecyl etherification of XG as a means of enhancing solubility of glibenclamide through polymeric micellization process. The copolymer provided 122-fold higher aqueous solubility than pristine drug. The micelles had a command on the drug release in simulated biological fluids up to 8 h and on diabetes in alloxan-induced hyperglycemic rabbit model. The enmeshing of drug-loaded copolymer micelles into O-carboxymethyl aluminium xanthan hydrogel particles declined drug release rate in simulated fluids. They discerned better hypoglycemic activity of glibenclamide after trapping micelles into carboxymethyl XG hydrogels. The glucose-lowering action lasted up to 8 h in alloxan-induced hyperglycemic rabbits.124 Quan et al.125 conjugated hexdecyl groups to XG under its ordered conformation, where its structure remains altered. Intriguing to note that, this derivative associated at a very low concentration (0.16%) in water, and showed better thermal resistance, and 4-fold higher viscosity. Altogether the hydrophobic modification of XG under order conformation contributed significantly to these changes in XG properties.125
The substitution of 4- or 8-tetradecyl chains to XG assisted in denser association of the polymer network, resulting in higher solution viscosity. Greater hydrophobic interaction amongst the polymer chains was presumed for this close association at higher polymer concentration and alkyl substitution, though the temperature had a negative impact126 (Fig. 4).
Bakshi et al.127 found that solid dispersion prepared by hot melt process in combination with microwave irradiation resulted in 75-fold increase in glibenclamide solubility and better preclinical hypoglycemic activity at a drug
:
Soluplus® ratio of 1
:
7. This observation invigorated them to incorporate the solid dispersion into carboxymethyl XG mini-matrices in order to circumvent the fluctuations in dissolution rate associated with pure drug under gastrointestinal fluids. Carboxymethyl XG matrices containing Soluplus gradually released the drug up to 70% till the end of 8 h without any burst effect. On contrary, XG matrices showed burst release of drug and corresponded to 100% in 6 h. It was noteworthy that the solubility enhancement caused by Soluplus dispersion was about 50-fold lower than that reported for hexadecyl xanthan copolymer.127
Ahuja et al.128 proceeded with synthesis and physical characterization of the carboxymethyl XG. They reported globular shape morphology and crystalline nature of carboxymethyl XG particles. The viscosity deteriorated after carboxymethylation. Carboxymethyl XG matrices revealed faster release of diclofenac sodium compared to unmodified XG. For brevity, the carboxymethyl XG matrices emptied its entire content in 3 h; while unmodified XG released half of its content in 16 h. It was postulated that less viscous carboxymethyl XG promoted penetration of water into the matrix, caused faster dissolution of the matrix resulting in faster drug release in phosphate buffer solution (pH 6.8). However, the release profiles of diclofenac-loaded carboxymethyl XG matrices were contradictory to that reported by Bakshi et al.127
Munir et al.129 reported better thermal stability and DPPH free radical scavenging (antioxidant) activity of XG after carboxymethylation. The antibacterial effects of gum became intensified after modification. In another study, carboxymethyl XG capped gold nanoparticles showed their unique excellence in cancer cell killing. Microwave synthesis of carboxymethyl XG-capped gold nanoparticles containing doxorubicin exhibited about 4.6-folds higher anticancer efficacy in vitro in presence of an ionophore (i.e. nigericin) than free doxorubicin.130
The O-carboxymethyl ether derivative of XG was largely synthesized for the fabrication of ionically and/covalently crosslinked hydrogel particles and tested for controlled drug delivery. The outcomes of such investigations are summarized in Table 1.
| Type of devices | Polymers/cross linkers | Research outcomes | References |
|---|---|---|---|
| PEC hydrogels | Chitosan and XG/Opadry | • Incorporation of metronidazole into pre-formed hydrogels in significant amount is possible by diffusion technique | 131 |
| • Hydrogels swell less in simulated gastric medium | |||
| • Enteric coating allowed 50% drug for release in colonic pH | |||
| PEC hydrogels | N-Trimehtyl chitosan (TMC)/carboxymethyl xanthan gum (CMXG) | • Encapsulation efficiency of ciprofloxacin reached to about 93.8% at higher drug load | 132 |
| • Drug-loaded hydrogel was highly effective against the Gram positive and Gram negative bacterial strains | |||
| • Highest diameter of inhibition zone against Escherichia coli as compared to gentamicin | |||
| • Highest cell viability (97%) in lung human normal cell lines was noted at concentration up to 50 μg mL−1 | |||
| Ionic and polyelectrolyte complexation | Polyethyleneimine (PEI)/CMXG/AlCl3 | • Increasing PEI (0.5–2%) and exposure time (5–30 min) decreased drug entrapment efficiency from 96.50 to 77.50% and from 92.25 to 70.37%, respectively | 133 |
| • PEI treatment reduced swelling of the beads | |||
| • Depending on formulation variables, 40% and 80% drug released in 2 h in pH 1.2 and in 5–6 h in pH 6.8, respectively | |||
| • PEI treated diltiazem–resin complex beads released the drug following non-Fickian transport mechanism | |||
| • Bioavailability was 1.59 times higher with PEI-treated formulation than pure drug solution in rabbit model | |||
| • Data showed good in vitro–in vivo (IVIVC) correlation | |||
| Magnetically responsive polyelectrolyte complex hydro-gels | XG and chitosan in the presence of iron oxide magnetic nanoparticles (MNPs) using D-(+)-glucuronic acid δ-lactone as a green acidifying agent | • Incorporation of Fe3O4 MNPs (8 nm size) into complex hydrogels induced porosity and greatly improved mechanical properties and storage modulus | 134 |
| • Magnetically responsive hydrogels improved NIH3T3 fibroblasts cell proliferation and adhesion in an external magnetic field relative to pristine hydrogels without MNPs in vitro | |||
| • Suitable for use as a magnetically stimulated system in tissue engineering applications | |||
| Tablets | Polyethylene glycol/XG/chitosan | • Drug release profiles of tested metronidazole tablets and commercial ER formulation were similar in 0.1 M HCl and phosphate buffer pH 6.8 | 135 |
| • Bioadhesion of tested tablets was three times higher than commercial tablets to sheep duodenum | |||
| • Absorption of metronidazole from test product was faster than that of commercial product with a maximum plasma level attained at 4.37 and 6.14 h, respectively | |||
| Interenetrating network (IPN) hydrogel beads | CMXG and carboxymethyl cellulose/AlCl3 | • Methacrylic acid-based ion exchange resins (IER) were synthesized using ethylene glycol dimethacrylate, N,N′-methylene bis acrylamide, and divinyl benzene coded as ME, MB and MD respectively | 136 |
• IER : ofloxacin ratio of 1 : 2 provided highest drug loading ∼98% MD and MB; however, the same was ∼85% for ME |
|||
• Taste masking studies at salivary pH 6.8 showed that MD : ofloxacin (1 : 4) showed lowest (1.22%) release of drug for a contact time of 30 s than others |
|||
| • Presence of bulky divinylbenzene imparted steric hindrance for the exchange of phosphate groups with the amine groups present in drug at salivary pH, ultimately resulting in slow release of the drug | |||
• CMXG beads containing MD : ofloxacin (1 : 4) (636 μm) had highest drug entrapment efficiency of 91.90% following treatment with 2% AlCl3 |
|||
• MD : ofloxacin (1 : 4)-carboxymethyl XG/carboxymethyl cellulose IPN beads (1122 μm) had 90.23% drug entrapment efficiency |
|||
• Compared to gastric pH, drug release from MD : ofloxacin (1 : 4)-carboxymethyl XG beads and carboxymethyl XG/carboxymethyl cellulose IPN beads at intestinal pH 7.4 became prolonged and extended up to 10 h |
|||
| IPN hydrogel beads | Casein and CMXG/aluminium chloride/glutaraldehyde | • Glutaraldehyde treatment prohibited extent of degradation of hydrogels in pH 7.4 phosphate buffer containing 0.2% lysozyme | 137 |
| • Theophylline release was slower in pH 1.2 buffer solution than in pH 6.8 buffer | |||
• Increasing carboxymethyl XG : casein ratio decreased the extent of drug release marginally both in acidic media and alkaline media in 2 h |
|||
• Higher carboxymethyl XG : casein ratio and drug loading improved drug entrapment efficiency from 28.6 to 53.81% and from 53.81% to 83.59%, respectively |
|||
| • Increase in glutaraldehyde concentration caused lowering of drug entrapment efficiency from 83.01 to 40.03% upon 15 min exposure. Reduction of exposure time to 5 min increased DEE to 85.12% | |||
| • Theophylline transformed into amorphous state after entrapment | |||
| • Shifting of pH of dissolution medium from 1.2 to 6.8 caused significant swelling of beads | |||
| • Increase in AlCl3 concentration (2–8%) increased swelling of beads by 10.26% and 11.62% in pH 1.2 buffer and pH 6.8 buffer solutions, respectively | |||
| IPN hydrogel beads | Pectin/CMXG/Al3+ ions and covalent cross-linking with glutaraldehyde | • Both swelling and drug release were relatively low in pacidic medium than in pH 6.8 buffer | 138 |
| • In vitro delivery of diltiazem was dependent upon the extent of cross-linking and amount of drug used in the IPN hydrogel beads | |||
| IPN hydrogel beads | CMXG and sodium alginate/AlCl3 | • Cmax was significantly less and Tmax (2.91 ± 0.5) was relatively higher from the drug loaded IPN beads than those from the control and reference in rabbit model | 139 |
| • Relative bioavailability of test formulation was 109.02% and 112.79% compared to control and reference, respectively | |||
| Compression coated tablets | CMXG and sodium alginate/CaCl2 | • Compression-coated tablets of Ca2+ ion crosslinked CMXG and sodium alginate could deliver prednisolone without the need of colonic bacterial intervention for degradation of the polysaccharide coat | 140 |
• Blend of CMXG and alginate (1.5 : 3.5) provided Tlag of 5.12 h and Trap (time required for immediate release following Tlag) of 6.50 h |
|||
| Hydrogel beads | CMXG/AlCl3/glutaraldehyde | • Diltiazem–cation exchange resin was loaded into carboxymethyl XG hydrogel beads | 141 |
| • Sequential cross-linking involving glutaraldehyde treatment of ionically preformed hydrogel beads produced smaller beads with higher drug entrapment efficacy (86.52%) and prolonged release characteristics than ionic cross-linking, and simultaneous ionic/covalent cross-linking | |||
| • Swelling of the beads was higher in acid solution of pH 1.2 than in buffer solution of pH 6.8 | |||
| • Burst release (∼50%) in acid solution, followed by extended release up to about 7 h | |||
| Tablets | CMXG/CaCl2 | • Increase in degree of calcium co-ordination/cross-linking reduced swelling of Ca–CMXG matrix tablets compared with carboxymethyl XG matrix | 142 |
| • Erosion of Ca–CMXG matrices was higher than CMXG matrix | |||
| • Release of prednisolone from Ca–CMXG matrices containing upto 33.33% (w/w) CaCl2 was less than that from CMXG matrix | |||
| • Release of drug from the matrix containing 50% (w/w) of CaCl2 was rapid and approached almost to that from CMXG matrix | |||
| IPN beads | Carboxymethyl cellulose and CMXG/AlCl3 | • Higher extent of cross-linking led to decreased particle size from 1080 to 1420 μm | 143 |
• Variation in cellulose to gum ratio from 1 : 1 to 2 : 1 dropped drug encapsulation efficiency of IPN beads from 96.96 to 77.45% |
|||
| • Drug entrapment efficiency of the beads decreased at higher salt strength | |||
| • Increase in salt strength from 4 to 8% slowed drug release rate in acidic and alkaline media | |||
| • Drug release continued up to 8 h in pH 7.4, indicating better intestinal drug release | |||
| Homopolymeric and IPN beads | CMXG and sodium alginate/AlCl3 | • Entire ibuprofen can be loaded into the beads with a maximum coefficient variation of 1.87% | 144 |
| • IPN hydrogel beads provided more sustained release of ibuprofen than homopolymeric beads | |||
| • Rapid drug release from Al–CMXG beads, accounting 42.5% release in 2 h | |||
| • Incorporation of higher amounts of alginate in IPN beads decreased drug release | |||
| • Release of drug from Al–alginate beads was the lowest, releasing 25.4% drug in 2 h in acidic medium | |||
| • Release of drug was the fastest from Al–CMXG in same duration | |||
| • Drug release from Al–alginate beads was faster than those from the IPN beads in pH 6.8 phosphate buffer | |||
| IPN beads | CMXG and sodium alginate/aluminium chloride | • Ulcerogenicity decreased significantly with ibuprofen-loaded IPN beads in comparison to the pure drug in adult male albino Wistar rats | 145 |
| Microparticles | CMXG/aluminium chloride | • CMXG or alginate-coated Al–CMXG microparticles were prepared | 146 |
| • Higher salt concentration decreased BSA entrapment efficiency of the uncoated microparticles from 86–61% | |||
| • BSA entrapment in coated microparticles was found lower (78–79%) than uncoated microparticles | |||
| • Uncoated microparticles released almost half of its content in NaCl–HCl buffer solution (pH 1.2) in 2 h | |||
| • Alginate and xanthan coated microparticles did not liberate a substantial amount of entrapped protein in acidic medium, rather prolonged protein release in PBS solution (pH 7.4) up to 10 and 12 h, respectively | |||
| • Sodium dodecyl sulfate–polyacrylamide gel electrophoresis indicated retention of protein integrity in the microparticles | |||
| Microparticles | CMXG/aluminium chloride | • Variation in pH of carboxymethyl XG solution did not affect protein entrapment and release significantly | 147 |
| • Increase in initial protein loading tended to increase protein release in buffer solution of pH 1.2 and in PBS solution (pH 7.4) | |||
| • Higher polymer concentration suppressed protein release substantially in both acidic and alkaline media | |||
| • Maximum 86.39% protein entrapment efficiency was noted | |||
| Hydrogel beads | CMXG/aluminium chloride | • Diltiazem–resin complex was loaded into CMXG beads | 148 |
| • Higher gelation period (5–20 min) and AlCl3 concentration (1–3%) decreased drug entrapment efficiency from 95 to 79% and 88.5 to 84.6%, respectively | |||
| • Gum concentration up to 2.5% improved drug entrapment efficiency to 90.7% | |||
| • Higher swelling was accounted for faster drug release in simulated gastric fluid than in intestinal fluid | |||
| Hydrogel beads | CMXG/aluminium chloride | • Viscosity of CMXG was always lower than that of XG | 149 |
| • Formation of discrete and spherical BSA-loaded microparticles were dependent on microenvironmental pH | |||
| • BSA entrapment efficiency was 82% | |||
| • Higher swelling contributed faster protein release in acidic medium than that in alkaline medium | |||
| • pH of the gum solution influenced the swelling and protein release considerably | |||
| Nanoparticles | XG/sorbitan monooleate/oleylamine | • XG-functionalised sorbitan monooleate/oleylamine nanoparticles had average diameter of 146.8 nm and high surface charge (−48 mV) | 150 |
| • Core–shell morphology of enhanced green fluorescent protein plasmid (pEGFP) loaded nanoparticles was evident | |||
| • Cytotoxicity and transfection capacity of nanoparticles were excellent in human umbilical vein endothelial cells (HUVECs) | |||
| • Pre-clinical study confirmed the potential of XG-functionalized span nanoparticles for gene targeting to endothelial cells | |||
| • Xanthan shell protected associated DNA from DNase degradation, a prerequisite for intact delivery of bioactives to its site of action | |||
| Layered Fe–XG hydrogels | XG/FeCl3 | • Fe3+-coordination enabled XG to form hydrogels under ambient temperature | 151 |
| • Fe–XG hydrogel exhibited a regular laminated structure under scanning electron microscope | |||
| • XG hydrogels possessed uniform layered structure, enhanced mechanical strength and excellent swelling behavior | |||
| • Sol–gel conversion of XG-based hydrogel could be realized by UV light in the presence of sodium lactate | |||
| • Sol–gel conversion ability of Fe–XG hydrogel could provide data for using as sensor to detect oxidizing or reducing agents, as an actuator under UV light with enough sodium lactate, or for the drug release in the future study | |||
| Floating hydrogel beads | Chitosan/XG | • Variation in chitosan to XG ratio did not affect glipizide release behaviors of the beads in phosphate buffer pH 7.4 up to 24 h | 152 |
| • Drug entrapment efficiency was 80–95% | |||
| • Beads possessed comparable buoyancy in gastric fluids and satisfactory bioadhesive strength | |||
| • Swelling kinetics differed significantly in pH 1.2 and 7.4 buffer | |||
| Hydrogel beads | CMXG/carboxymethyl cellulose/AlCl3 | • Beads released considerably less amount of aceclofenac in acid solution (maximum 14.2%) and provided controlled release in phosphate buffer solution (pH 6.8) | 153 |
| • Aceclofenac was compatible with the matrix | |||
| • Morphology, size and drug entrapment efficiency of beads, and in vitro drug release was affected by viscosity of polymer dispersion, initial drug load, and concentration of total polymer and AlCl3 |
Tao et al.157 endorsed sodium trimetaphosphate (STMP), a non-toxic and water soluble cyclic triphosphate for the crosslinking of hydroxy groups of XG chains under alkaline condition to design hydrogel disks. One phosphorous group intertwined two sugar rings of different XG chains (Fig. 6). STMP crosslinking endowed hydrogel disks more elasticity and mechanical stability than physical hydrogels. This esterification reaction induced porosity in the hydrogels, with a mean pore diameter of 114.5 ± 22.1 μm. However, the pore diameter dropped to 31.5 ± 5.5 μm at 5% (w/v) XG due to sufficient crosslinking of the matrix. XG–STMP hydrogels swelled rapidly in the first hour and attained equilibrium in PBS (pH 7.4) in 28 h. However, the hydrogel disk swelled faster in water than that in PBS and remained undissolved for more than 11 days. Regarding protein diffusion, the hydrogels recorded a slow, sustained diffusion of bovine serum albumin in PBS medium over 50 h depending upon STMP concentration. The least diffusion (∼28%) was evident at 5% STMP. STMP crosslinking perhaps introduced more anionic charges into XG, thus facilitating more water uptake by the hydrogels. Furthermore, the counter ions inside the XG–STMP hydrogels might increase the osmotic pressure and cause higher swelling.158
Shalviri et al.158 mingled gelatinized starch and XG in order to develop hydrogel films. STMP crosslinking produced continuous and homogeneous films with few micropores, even in absence of plasticizer. Higher STMP (20%) and XG (20%) levels speeded up the swelling of films in deionized water by 1.7-folds compared to that in phosphate buffer (pH 7.4). As usual, the gel mesh size became enlarged from 2.84 to 6.74 nm as swelling continues. The permeation of anionic drugs (ibuprofen sodium and sodium salicylate) through films was slower than neutral entities, thus demonstrating their potential for controlled release of ionizable drugs. Intermingling of a hyperbranched polysaccharide, extracted from the Pleurotus tuber-regium sclerotic, and XG followed by STMP-crosslinking ensued the formation of hydrogels that demonstrated shear-thinning behaviors, and improved mechanical stability. In addition, the hydrogels presented self-healing ability and controlled drug release property. The hybrid hydrogel had a storage modulus better than XG–STMP hydrogel.159
Bejenariu et al.160,161 highlighted the importance of STMP
:
XG ratio on the swelling and release of cationic dyes from the hydrogels. The hydrogels obtained at STMP
:
XG ratio of 10
:
1 swelled 20 times in pH 7.0 and entrapped 87.5% methylene blue. The hydrogels liberated more amounts of dyes in NaCl solution than in acid solution (pH 3.0). Overall, STMP-crosslinking supported XG hydrogels for cationic drug release.
The dehydration of hydrogel-like human nucleus pulposus and imbalanced stress distribution in the intervertebral disc causes degenerative disc disease. Thus, the regeneration of nucleus pulposus is the key to success for treating this. However, the avascularity and low mitotic activity of chondrocytes limits their successful treatment.162 In view of this, Leone and coworkers163 proposed STMP-crosslinked PVA
:
XG (4
:
1) hydrogels as a good substitute for nucleus pulposus.
Bueno et al.21 appraised citric acid as a natural crosslinker for the synthesis of XG hydrogel films (∼0.03 mm thick) (Fig. 7). They observed that citric acid produced porous, homogeneous films without nanofibrils, indicating its crosslinking efficiency. However, it reduced the mechanical strength of the films. The properties of citric acid-crosslinked hydrogels were comparable to those reported for xanthan–starch films.164 The swelling of hydrogels was significant at pH 10.0; however, the same was negligible at pH 2.0 and pH 6.5. The water absorption was initially controlled by quasi-Fickian diffusion mechanism; however switched to anomalous diffusion at later period. Perhaps, the disruption of ester bonds favored swelling of the films in basic medium. They further reported that XG chains could be intertwined by heating at 165 °C without the need of citric acid. In this case, the diffusion of water into hydrogels changed from quasi-Fickian to Fickian at later times. Heating brought about weaker crosslinking of XG chains. The nanofibrils (about 20–30 nm diameter) were evident on cryofractured hydrogel surface. Moreover, the hydrogels did not respond to pH variation promptly as was seen in case of citric acid-treated hydrogels, because they had more crosslinks to be hydrolyzed.
Circular dichroism confirmed the disordered conformation (coils) of xanthan chains in case of citric-acid crosslinked hydrogels; whereas the crosslinking by heating left XG in an ordered conformation (helixes) in the hydrogels.165 Under coil conformation, usually a larger number of carboxylate groups are exposed, thereby providing citric acid an opportunity to give birth to more ester linkages. The protein release behaviors from hydrogels were quite amazing. Isoelectric pH of protein and pH of release medium played a crucial role in protein release. For instance, the heat-treated hydrogels completed the delivery of BSA after 1 h over the pH range of 2–10; except at pH 4.8 close to its isoelectric point. In contrast, the release of lysozyme became very low at pH 7.0. This could be attributed to the electrostatic attraction between lysozyme and hydrogels. Both hydrogel films seemed efficient as carriers for proteins (lysozyme) having high isoelectric point. The hydrogels preserved native conformation of lysozyme after loading and thus could offer substantial bactericidal activity in wound dressings. Followed by this, Huang et al.166 designed novel wound dressing material exploiting citric acid-crosslinked transparent, porous XG films laden with silver nanoparticles (AgNPs). The nanocomposite films were non-cytotoxic to fibroblasts (L929) at <10 μg mL−1. The dressing prohibited the formation of biofilms, reduced the inflammatory reactions, and triggered angiogenesis of the granulation tissues in non-healing wounds, infected with methicillin-resistant S. aureus. The nanocomposites impeded immature release of AgNP in PBS solution and hence exhibited the antibacterial effect for more than 24 h.
In a study,167 glycerol was mentioned for chemical bonding of XG in a waterless or near-waterless environment at temperature >105 °C (Fig. 8). It was hypothesized that water generated during cross-linking reaction could catalyze the unwinding of double-helix of XG and provide more access to its functional groups and backbone for cross-linking. The crosslinking occurred at glycerol
:
xanthan ratio of <27.6. Higher xanthan
:
glycerol ratio imparted more hardness, swellability (>39 g water per g gel), dye sorptivity (>85%) to the hydrogels. The hardness was almost 40 times greater with 50% xanthan gel than that made with 5%. The interdiction of red 40 and blue 1 (food dyes) release in water (60–70% in 24 h) unfolded the possibilities for constructing slow-release matrices. Moreover, the crosslinked gels came up effectively with dye absorbent capacity; thus advocated its application in food, pharmaceutical and other industries.
Hamcerencu et al.168 described esterification of XG with an unsaturated acrylic acid or acid reactive derivatives (acryloyl chloride, maleic anhydride) followed by grafting with N-isopropylacrylamide. This resulted in thermo- and pH-sensitive hydrogels. Maleic anhydride presented higher reactivity towards primary hydroxy groups (C6) as compared to others. Higher temperature and reaction time had positive impact on the degree of substitution.
Mendes et al.169 evinced that palmitoylation of xanthan (xanthan
:
palmitoyl chloride = 1.7) expedited self-assembly of XG and furnished a compatible environment for cell microencapsulation. However, there was a dearth of physical stability to enclose cells and protect from immunotoxins. Subsequent membrane coating of the microcapsules with poly-L-lysine allowed permeation of sufficient oxygen and nutrients necessary for cell survival and proliferation (Fig. 9).
Bhatia et al.170 pointed out that thio-esterification of XG with mercaptopropionic acid and thioglycolic acid evoked better ex vivo mucoadhesion (Fig. 10). The extent of mucosal retention of metronidazole-loaded buccal pellets of XG–mercaptopropionic acid was less than XG–thioglycolic acid. Improved mucoadhesion of thiolated XG over native XG could be credited to the disulfide links between mucus and thiol groups. Nonetheless, the buccal pellets of XG–thioglycolic acid sustained the diffusion of metronidazole more effectively than XG–mercaptopropionic acid and native XG pellets. The degree of thiol substitution in XG–thioglycolic acid was 1.07 times higher than XG–mercaptopropionic acid. This could be responsible for variable ex vivo bioadhesion and in vitro release characteristics of the two conjugates.
In view of the potential toxicity of surfactants as suspending agents, Skender and groups171 synthesized three ester derivatives of XG using diphenylmaleic anhydride, phthalic anhydride, and epichlorhydrin–phenol and assessed the worth of these derivatives as dispersing agent for double-wall carbon nanotubes in water. Xanthan itself is a very poor dispersing agent for carbon nanotubes. However, these derivatives proved useful as stabilizer for suspension of carbon nanotubes (0.5%, w/w). Xanthan esterified with diphenylmaleic-and phthalic-esters successfully immobilized carbon nanotubes in very acidic media compared to that esterified with epichlorhydrin–phenol. Above pH 5.0, all the derivatives stabilized the suspensions effectively. Summarily, the presence of aromatic moiety in XG backbone was essential in dispersing carbon nanotubes in water via p–p stacking interaction.
A group of investigators synthesized succinoyl XG following reaction with succinic anhydride in presence of 4-dimethylaminopyridine catalyst at room temperature.172 Succinoyl XG turned into unflowable hydrogels at a very low strength (1.4% w/w), while the unmodified XG existed as flowable fluid at the same concentration.
In case of native XG, the hydrogel network is usually formed through physical entanglements. Succinoylation promoted the formation of secondary bonds, rendering more elasticity to the hydrogels. Further, the hydrogels responded to ionic strength and sustained the release of gentamicin for 9 days in PBS (pH 7.4). The hydrogels inhibited the formation of biofilm and demonstrated excellent bactericidal function in rabbit subcutaneous S. aureus infection model. As was evident from cytocompatibility study against human lens epithelial cells, the hydrogels supported cell adhesion; proliferation and migration at a dose of 1 mg g−1. Overall succinoylated XG hydrogels were propitious as drug delivery materials for antibacterial applications.
Guo and coworkers174 brought into play xanthan aldehyde as a crosslinker for producing transparent, UV-protective edible gelatin films. Increased C
N groups by Schiff's base formation greatly improved the hydrophobicity, mechanical properties and thermal stability of gelatin films. Paiva and colleagues175 exploited XG aldehyde as an adhesive for the natural cork stopper. The authors proclaimed that oxidized XG performed well due to the reaction of aldehyde groups with hydroxy groups on cork surface during high temperature drying. Ma et al.176 disclosed a new hydrogel system based on XG aldehyde and phosphatidylethanolamine liposome. The hydrogel was sensitive to stimuli like heat, pH, and histidine and papain enzyme. The hydrogels manifested self-healing ability and provided an excellent environment for cell encapsulation for tissue engineering.
Intrinsic healing property of hydrogels is of utmost importance for in vivo drug delivery because this property could relieve hydrogels from destabilization under adverse mechanical or chemical exposure in vivo.177 Salazar and associates178 reported intrinsic self-healing ability of a composite hydrogel system of oxidized XG and chitosan. The hydrogels extended successful self-healing ability at room temperature and pressure while maintaining a good mechanical strength at equal chitosan
:
aldehyde XG mass ratio.
Injectable hydrogels have been abortive due to their instability to tissue exudates and delayed gelation under physiological conditions. Huang et al.179 attempted to overcome these issues. They devised a stable and rapid gelation method for fabricating self-healing hydrogels based on hydrogen-bonding interaction and Schiffs base reaction between XG aldehyde and carboxymethyl chitosan (Fig. 11). The incorporation of vascular endothelial growth factor (VEGF) in hydrogels speeded up the reconstruction of abdominal wall in rats. The hydrogel managed the release of protein effectively.
The antioxidant activity of oxidized XG was also disclosed in the literature. Xiong et al.180 exposed that XG when oxidized under alkaline medium exhibited better antioxidant activity than native XG. XG oxidized under acidic condition but having similar molecular weight had relatively poor antioxidant activity. The variable contents of pyruvate and reducing sugar could be responsible for this discrepancy. Nevertheless, dialdehyde XG could serve as a reducing agent for the synthesis of silver nanoparticles as well as designing biocompatible composite dressings suitable for burn healing.181
However, the study findings on emulsion containing octyl xanthan (disorder conformation) thwarted emulsion stability through creaming, regardless of its concentration. The instability problem became more pronounced at higher grafting density. However, this phenomenon reversed for n-hexadecylamine XG (disorder conformation).185
Bejenariu et al.161,186 reported a new XG hydrogels based on adipic acid dihydrazide (ADH) treatment. The crosslinking of XG with ADH is displayed in Fig. 13a. In the crosslinking reaction, LiNO3 was used for the stabilization of the helicoidal structure of XG at pH 3.0. The hydrogels exhibited pH-dependent swelling but the pH-effect was not so drastic. The least degree of swelling was noted at pH 3.0 because the helical conformation of XG predominated in crosslinked networks. Despite the prevalence of coil conformation, the weak amide bonds restricted the networks from exhibiting similar swelling behaviors at pH 13.0 to that noted under acidic condition. Notably, the highest degree of swelling was recorded at neutral pH. The hydrogels absorbed ∼98% of methylene blue in 24 h and released the dye in salt solution at a rate faster than in acidic solution (pH 1.5). Laffleur and groups187 showed that thiolated XG disc worked better in terms of stability (1.62-fold), ex vivo buccal mucoadhesion (8.35-fold) and tensile strength (2.65-fold) compared to unmodified xanthan. These findings coupled with its non-cytotoxicity towards Caco-2 cells inspired the authors in developing buccal patch to treat sialorrhea, a buccal disease associated with an involuntary loss of saliva. To fight against enhanced psychosocial and mental problems of sialorrhea patients,188 tannic acid was found suitable for inhibition of excessive flow of saliva. Laffleur et al.189 developed L-cysteine-conjugated XG buccal patch for tannic acid. The constant swelling in simulated saliva solution (pH 6.75) and non-cytotoxicity to Carey 24 cell lines embellished the buccal patch. Thiolation prohibited matrix erosion about five times and lessened the saliva flow about 33% more than the unmodified XG in excised porcine buccal mucosa. Mucoadhesive and water vapor uptake properties of XG became more pronounced after thiolation of XG. The patch released tannic acid half as fast as XG in 6 h in simulated saliva solution and thus opened an avenue for sialorrhea research. Menzel et al.190 adopted a distinct strategy for thiolation of XG. The process comprised of coupling reaction of 2-mercaptonicotinic acid (MNA) to L-cysteine by disulfide exchange and direct attachment to XG via carbodiimide mediated amide bond formation (Fig. 13b). XG-cysteine–MNA concurred about 1.7-fold and 2.5-fold higher mucoadhesion than cysteine-XG (XG-Cys) and XG ex vivo, respectively. In the presence of H2O2 oxidizing agent, XG-cysteine–MNA showed high stability towards oxidation. Reversible ciliary beat frequency in porcine nasal epithelial cell culture indicated low toxicity of all xanthan derivatives. The in situ gelling behavior of XG-Cys–MNA was independent of polyvalent cations, thus hinted safe application of aqueous solutions.
Mendes et al.191 synthesized an amphiphilic XG following conjugation of phospholipid (1,2-dioleoyl-sn-glycerophosphoetilamine, DOPE) to the anionic XG (Fig. 14). Considering two carboxy groups in xanthan repeating unit, the degree of substitution was estimated to about 1.16 ± 0.024. The investigators applied microfluidic approach for the production of microcapsules for cell entrapment. Coating with 0.1% poly (L-lysine) improved the mechanical strength of the capsules. The viability of ATDC5 cells remained unaltered after encapsulation. The droplets generated through microfluidic approach and the self-assembly of xanthan–DOPE produced microcapsules with an environment compatible for cell survival and proliferation.
The antimicrobial activity of lysozyme is limited to Gram positive bacteria, but its antibacterial spectrum can be extended towards Gram negative bacteria after carbohydrate conjugation through the Maillard reaction. Hashemi et al.192 synthesized xanthan gum-lysozyme (1
:
1) conjugate under mild Maillard reaction condition (sodium phosphate buffer, pH 8.5 and 60 °C for 10 days). It was found that approximately 1.9 mmol XG could be attached to one mole lysozyme. Lysozyme–XG conjugates showed pH- and temperature-dependent solubility, and heat stability with improved emulsion and foaming properties. The lysozyme conjugation significantly impeded the growth of Staphylococcus aureus and Escherichia coli in a dose dependent manner. These findings broaden the application of this enzyme in food or pharmaceuticals.
:
PVA ratio and crosslinker concentration, the microparticles showed 84% drug entrapment efficiency. The crosslinker concentration declined the rate of delivery of entrapped diclofenac molecules considerably in vitro. On contrary, XG promoted the drug release rate in biological fluids. Preclinical trials demonstrated higher relative bioavailability (1.69 times) having a good in vitro-in vivo correlation. The pioneering work of Ray et al.193 enlightened us on the potential utility of glutaraldehyde as a crosslinker for XG for controlled drug delivery applications. However, the toxicity profile of glutaraldehyde poses a major concern which perhaps precludes its use as chemical crosslinker for drug delivery matrices (Fig. 15).
:
XG ratio of 12
:
8. Additionally, the apparent viscosity and shear thinning characteristics of XG progressively increased at higher strength. At higher XG content, more hydrophilic groups entangled into regular network structure by hydrogen bonding and van der Waals forces, which enabled wrapping of more free water. Consequently, the viscosity of the composite solution became larger and pseudoplasticity came into existence.198 The PVA–XG (12
:
8) hydrogels swelled abruptly at high pH and attained a maximum equilibrium swelling index of 1.3 at pH 8.0. This indicated that alkaline pH favored the adsorption of methylene blue by composite hydrogels. XG contributed to the improved swelling of PVA–XG hydrogels; however reduced the compression properties owing to the formation of hydrogen bonds between polymers. Ultimately, the mechanical properties of the hydrogel diminished. The maximum adsorption of methylene blue dye was noted at PVA
:
XG ratio of 12
:
8. A strong electrostatic attraction between XG and dye could contribute to this effect. The recycling ability of hydrogels strongly supported its application in dye removal from waste water. Shimizu et al.199 observed that the addition of 0.2% XG in 17% PVA solution minimized liquid viscosity while maintaining mechanical properties and pourability into injection molds during the fabrication of 3D models. The addition of XG facilitated the fabrication of biomodels through gelation of PVA/XG solution in water
:
DMSO (20
:
80) at −30 °C for 24 h. Bhunia and coworkers200 prepared PVA (10%)
:
XG (1–5% w/w) hydrogel films following irradiation at 5 kGy dose under high energy electron beam and investigated the influence of low molecular weight (1.4 kDa) PVA (LPVA) and high molecular weight (11.5 kDa) PVA (HPVA) on the physical and mechanical properties of the film. The physical properties of the films under dry state remained indistinguishable but HPVA–XG hybrids were superior in terms of wet-mechanical properties and diltiazem release. Tensile strength of HPVA–XG films was excellent at 1% XG and the same was much less in LPVA–XG films. The degree of swelling became intensified with increasing XG content in HPVA hydrogels.
In LPVA–XG hydrogels, the swelling dropped drastically on addition of 1% XG, but eventually increased at 3% and 5% XG concentration. Thus, the most physico-mechanically balanced hydrogel membranes were obtained at 1% and 5% XG for HPVA and LPVA, respectively. A sharp loss in crystallinity in presence of 1% XG indicated huge loss of cohesive interaction and establishment of higher HPVA–XG interaction. On contrary, gradual increase in XG content up to 5% produced greater crystallinity in LPVA hydrogels. LPVA was surprisingly more viscous than HPVA201 and hence, LPVA–XG produced better phase compatibility, particularly at higher XG content. On contrary, intermingling of HPVA and XG generated better phase mixing at low XG content but led to huge phase separation at elevated XG level due to viscosity mismatches. LPVA showed better phase mixing with 5% XG. In HPVA
:
XG (1%) films, the diltiazem molecules were not uniformly distributed because of their different phase viscosity, thus failed to retain drug appreciably alike LPVA
:
XG (5%) films. The drug–PVA–XG hydrogen bonding interaction dictated the entrapment of diltiazem within PVA–XG hybrid. High flexibility in LPVA
:
XG (5%) thus allowed more diltiazem to elute in swelled state despite their better drug entrapment efficiency than HPVA
:
XG (1%) films. Regardless of XG concentration, the drug release was insignificant (2.5–4.6% in 12 h). The investigators achieved success in suppressing the burst release of drug from PVA hydrogels following exposure to irradiation. Disha et al.202 prepared hydrogels by heating XG, sodium benzoate, and potassium sorbate and glycerin mixture at 85 °C. The biodegradability characteristics of XG persisted over the concentration range of 2–3%. The hydrogels were devoid of antimicrobial activity against E. coli and Klebsiella spp. The physical crosslinking (H-bonding interactions) of XG with poly (N-vinyl imidazole) enabled Sabaa and coworkers203 to fabricate hydrogels containing bovine serum albumin (BSA). Depending on variation in gelation time, BSA loading and polymer concentration, the protein entrapment efficiency escalated to 99.17%. Higher polymer concentration promoted BSA release in PBS. The biocompatibility of hydrogel was ascertained on VERO cell line. SDS-PAGE analysis confirmed the structural integrity of protein after encapsulation or release.
Intra-articular injection of hyaluronic acid could be effective in treating osteoarthritis due to its lubricating and cushioning properties.204,205 However, hyaluronic acid rapidly degrades in vivo by hydrolytic or enzymatic reactions.206 Henceforth, a polymer which is similar to hyaluronic acid in structure and function, but with a longer effect in the joint is needed. XG is similar to hyaluronic acid in rheology and viscosity.207 Additionally, XG solution is very stable in a wide range of pH, ionic strength and temperature.208 XGlyase is mainly produced by bacterium;209 therefore XG is not easily degraded in vivo. Intra-articular injection of XG could be an effective therapy for osteoarthritis. Han et al.210 extensively purified XG, dissolved in buffered physiological saline and sterilized at 121 °C for 15 min and evaluated the protective effect of XG injection on articular cartilage. Results indicated that injection of XG could protect the joint cartilage and reduce papain-induced osteoarthrotis progression in rabbit model. The same result was obtained at an injection frequency lower than HA. This finding seemed promising in the development of a new therapeutic method for osteoarthritis. Bueno et al.65 synthesized XG–hydroxyapatite particles following homogenization of XG solution with Ca(OH)2 and H3PO4 solution under pH 7.5. Similarly, xanthan strontium-substituted hydroxyapatite particles were obtained using Ca(OH)2, Sr(CH3COO)2, xanthan solution and H3PO4 solution at pH 7.5. Initially Ca2+ ions were dissolved at pH 10.0 in presence of xanthan chains. Calcium ions were chelated by xanthan chains, forming nucleation sites for hydroxyapatite crystal growth. As phosphoric acid was added to the solution, the medium pH decreased to ∼7.5, promoting the precipitation of Ca2+ ions as hydroxyapatite. XG–hydroxyapatite and xanthan strontium-substituted hydroxyapatite nanoparticles presented mean size of 56 ± 18 nm and 75 ± 18 nm, respectively. Xanthan aqueous solution containing nanoparticles was casted into xanthan-based nanocomposite hydrogels in presence of citric acid. The dehydration crosslinking was accomplished by heating the films at 165 °C for 7 min. The nanocomposite films were apparently homogeneous. Hence, the presence of xanthan chains on the surface of particles provided an indication of compatibility between particles and xanthan chains. Nanocomposites presented porous structure and the incorporation of Sr or xanthan–hydroxyapatites did not affect the surface energy and consequently, posed no substantial influence on osteoblast proliferation. On the other hand, the chemical composition of nanocomposites influenced ALP activity. ALP is a cell membrane glycoprotein that catalyzes the hydrolysis of phosphate esters in alkaline pH and thus plays an important role in the mineralization process of bone matrix. Its activity in human serum is used as indication for diseases related to liver and/or bone. It was noted that the osteoblast ALP activity increased as the filler content was increased from 10% to 30% in both the nanocomposites, but this enhancement was much more pronounced in case of citric acid crosslinked XG–strontium hydroyapatite. In fact, the presence of strontium in hydroxyapatite structure supported osteoblast and osteoclast growth. Nanocomposites made of crosslinked xanthan chains and xanthan hydroxyapatite (10%) was homogeneous and mechanically stronger than bare xanthan networks or nanocomposites with hydroxyapatites. Mixing of ZnO nanoparticles (size 15–25 nm) with XG–PVA mixture followed by irradiation at 30 kGy led to the generation of biocompatible XG–PVA/ZnO nanocomposite dressing hydrogels.211 Homogeneous porous hydrogel network and the presence of ZnO nanoparticles provided an excellent fluid uptake capacity in pseudo-extracellular fluid (554–664%) and water (1281–1603%). The water retention capacity (about 50–65% after air exposure for 6 h) and water vapor transmission rate (167–184 g m−2 h−1) was sufficient to keep wound's surface moist. ZnO dressings exhibited profound antimicrobial activity against Staphylococcus aureus, Escherichia coli and Candida albicans. To avoid lumps and accelerate the dissolution of XG in water, Zhao et al.212 modified the surfaces of XG particles in dimethylbenzene with organometallic complex COMe at pH 4.5 adjusted by citric acid. The modification didn't change the molecular structure of XG; however weakened the hydrogen bonding interaction between XG molecules. Dispersible XG powders were completely dissolved in simulated seawater in 35 min without lumps. It was reported that sequential control of wetting and drying of XG produced sticky samples, thus posed difficulty in handling.213 Co-grounding of this treated XG with mannitol (1
:
1) improved the flowability and crystallinity marginally. Co-grounding afforded excellent water loading capacity (60.93%) and thus appeared to be an effective disintegrant for roxithromycin orodispersible tablets. The modified XG (10% w/w) and microcrystalline cellulose (MCC) (15%) allowed the disintegration of tablets in less than 60 s. At 1
:
3 ratio of co-grounded XG
:
microcrystalline cellulose, the tablets even disintegrated in about 14 s. The tablets reduced the lag time 9-fold and remained stable over a period of 12 months. Highly porous structure of modified XG and higher level of MCC promoted faster wetting (6.52 ± 0.42 s) and water absorption (150%). A marginal difference in drug release was noted at salivary pH (pH 6.4) and physiological pH (pH 7.4) (∼91–93% in 30 min). Higher percentage of drug release could provoke drug absorption through buccal cavity. Above all, the modified XG behaved like a directly compressible excipient and exhibited swelling dynamics suitable for use in rapidly disintegrating tablets.
The acetalated XG hydrogels improved the pharmacokinetics of entrapped drug remarkably. The physical treatments such as extrusion, freezing–thawing and high shear homogenization greatly improved the mechanical properties of XG. In addition, the physically crosslinked XG hydrogels had immense potential in encapsulating proteins without alteration of its structural integrity. The intra-articular injection of purified XG on articular cartilage was found effective as well against osteoarthritis. The XG-based nanocomposites had shown excellent mechanical stability, osteoblast ALP activity as well as wound dressing capability. Even, simple co-grounding of XG with mannitol caused reasonable improvement in flow characteristics of XG. Overall, the findings suggested that the functionalized XG had great potential for pharmaceutical and biomedical applications. However, the in vivo potential of these novel XG derivatives are yet to be assessed explicitly in order to unveil their safety and efficacy towards drug delivery and biomedical applications. This review would certainly encourage the pharmaceutical and biomedical researchers to explore other polysaccharides for developing newer materials for commercial use.