Open Access Article
Van Manh Tien‡
a,
Van Hoang Ong‡ac,
Tuyet Nhung Pham
*a,
Nguyen Quang Hoad,
Thi Lan Nguyene,
Pham Duc Thangab,
Le Khanh Vinhf,
Pham Thi Nhat Trinhh,
Doan Thi Ngoc Thanhi,
Le Minh Tung*g and
Anh-Tuan Le
*ab
aPhenikaa University Nano Institute (PHENA), Phenikaa University, Hanoi 12116, Vietnam. E-mail: nhung.phamthituyet@phenikaa-uni.edu.vn; tuan.leanh@phenikaa-uni.edu.vn
bFaculty of Materials Science and Engineering, Phenikaa University, Hanoi 12116, Vietnam
cUniversity of Transport Technology, Trieu Khuc, Thanh Xuan District, Hanoi, Vietnam
dFaculty of Physics, VNU University of Science, Vietnam National University, Hanoi, 334 Nguyen Trai, Thanh Xuan, Hanoi, Vietnam
eInternational Training Institute for Materials Science (ITIMS), Hanoi University of Science and Technology (HUST), 01 Dai Co Viet Road, Hanoi, Vietnam
fInstitute of Physics at Ho Chi Minh City, Vietnam Academy of Science and Technology (VAST), Ho Chi Minh 70000, Vietnam
gDepartment of Physics, Tien Giang University, My Tho City, Tien Giang Province, Vietnam. E-mail: leminhtung@tgu.edu.vn
hDepartment of Education and Basic Science, Tien Giang University, My Tho City, Tien Giang Province, Vietnam
iDepartment of Agriculture and Food Technology, Tien Giang University, My Tho City, Tien Giang Province, Vietnam
First published on 3rd April 2023
The electrochemical behavior and sensing performance of an electrode modified with NiFe2O4 (NFO), MoS2, and MoS2–NFO were thoroughly investigated using CV, EIS, DPV, and CA measurements, respectively. MoS2–NFO/SPE provided a higher sensing performance towards the detection of clenbuterol (CLB) than other proposed electrodes. After optimization of pH and accumulation time, the current response recorded at MoS2–NFO/SPE linearly increased with an increase of CLB concentration in the range from 1 to 50 μM, corresponding to a LOD of 0.471 μM. In the presence of an external magnetic field, there were positive impacts not only on mass transfer, ionic/charge diffusion, and absorption capacity but also on the electrocatalytic ability for redox reactions of CLB. As a result, the linear range was widened to 0.5–50 μM and the LOD value was about 0.161 μM. Furthermore, stability, repeatability, and selectivity were assessed, emphasizing their high practical applicability.
For the aim of enhancing the inherent characteristics, many spinel ferrite-based nanocomposites have been fabricated for boosting their diversity applicability from environmental, biomedical, and sensors to biotechnology applications.18–21 Among them, MoS2/NFO has been considered a highly promising nanocomposite for many different applications. Benefiting from possessing a large surface area and impressive structure with three atomic layers S–Mo–S stacked by van der Waals forces, MoS2 layers could support the effective dispersion of NFO nanoparticles (NFO NPs).22–24 Besides, owing to the presence of two different components within a structure, NFO NPs remarkably prevented the aggregation of MoS2 layers, leading to better connections and interactions between MoS2 and NFO as well as creating a larger active surface area. Accordingly, MoS2–NFO has been used as a potential candidate for electrochemical supercapacitors, catalysis, and energy conversion applications.25 For instance, M. Karpuraranjith et al.26 reported MoS2–NFO as an efficient dual-functional hybrid catalyst for the oxygen evolution reaction and degradation of dye pollutants. Yan Zhao et al.27 also developed NFO–MoS2 composites with great synergistic effects, which offered a higher-performance supercapacitor, compared with that of individual MoS2 sheets and NFO NPs, respectively. In another research, Wenzhi Fu et al.28 demonstrated the enhanced visible-light photocatalytic activities in the NFO–MoS2 structure.
However, as far as we know, the greater insight into the electrochemical characteristics and sensing performance of NFO–MoS2-modified electrodes has been not still explored while it is one of the essential goals in opening new opportunities for novel applications of not only NFO–MoS2 but also spinel ferrite-based nanomaterials. As known, NFO–MoS2 nanocomposites possess many advantages, which are very beneficial for electron transfer reactions, electrochemical behaviors, and electrocatalytic activities including large active surface area, high electronic conductivity, good redox chemistry, and potential electrocatalytic. Such merits promise to provide outstanding electrochemical properties and performance for NFO–MoS2-modified electrodes. In this work, NFO, MoS2, and MoS2–NFO nanocomposites were prepared using simple methods including hydrothermal and probe sonication methods, aiming to modify the working electrode surface of commercial screen-printed electrodes (SPEs). The electrochemical characteristics and sensing performance towards clenbuterol (CLB) detection of the proposed electrodes were thoroughly investigated. Among modified SPEs, MoS2–NFO (2
:
1)/SPE exhibited impressive electrochemical properties and sensing performance compared with other modified electrodes. Particularly, as demonstrated in our previous reports, the positive effect of the presence of the external magnetic fields on electrochemical behaviors and sensing performance was demonstrated.29–32 Herein, the influence of external magnetic field (MF) on the MoS2–NFO (2
:
1)/SPE was also further evaluated, contributing to optimizing the new research in the future.
+ Working electrode: carbon (4 mm diameter).
+ Auxiliary electrode: carbon.
+ Reference electrode: silver or Ag/AgCl.
:
1 and 1
:
2. Finally, the above-mixed solutions were ultrasonicated for 20 min.
000 Hz, all electrodes were continually executed by electrochemical impedance spectroscopy (EIS) measurement.The second, CV and DPV were measured on the bare SPE and modified SPE in the presence of CLB without and with MF. CV measurements were performed at a scan rate of 70 mV s−1 in the potential range from −0.3 to 0.6 V, potential step = 0.01 V. Meanwhile, DPV measurements were also carried out as following conditions: scan rate of 6 mV s−1, Epulse = 0.075 V, Tpulse = 0.25 s, Tequilibrium = 120–200 s and pH difference.
cos
θ, with kS as Scherrer constant and β is full width at half maximum of peak 2θ = 19.5° (Fig. S1d†). The XRD pattern of MoS2–NFO nanocomposites was recognized in Fig. 1c and zoomed in Fig. 1c′, one can see two well-defined broad peaks at 39.5° and 49.7°, belonging to (103) and (105) planes of MoS2. Meanwhile, the presence of other low peaks could be featured in XRD diffraction of NFO NPs within MoS2–NFO nanocomposites, indicating the co-existence of both MoS2 sheets and NFO NPs within the MoS2–NFO nanocomposites. More importantly, the effective combination between NFO NPs and MoS2 did not cause any change in the crystal structure of components.
![]() | ||
| Fig. 1 (a–c) XRD spectrum of NFO, MoS2, MoS2–NFO and (c′) the zoomed image of MoS2–NFO, respectively. | ||
Fig. 2 illustrates SEM images of NFO NPs, MoS2 sheets, and MoS2–NFO nanocomposites. As can be seen from Fig. 2a, the morphology of the NFO sample displayed nanoparticles with hexagonal plate-like morphology and uniform small size. By using ImageJ software, the size of NFO was accurately estimated to be 125 nm. In Fig. 2b, it is obvious that the MoS2 sample was composed of two-dimensional ultrathin sheets, distributed randomly with around 1.15 μm dimension. For the MoS2–NFO nanocomposites sample, it can see the small NFO NPs were dispersedly interlaced on the MoS2 sheets by forming heterojunctions, indicating NFO and MoS2 were completely combined with each other with slight aggregation due to the strong magnetism of NFO NPs. By stacking NFO-NPs among 2D-MoS2 materials through non-covalent van der Waals interactions, it displays the metallic–metallic contact without any other chemical bonds. It is suggested that the metallic nuclei in NFO with a strong affinity towards valency-deficient S atoms were preferentially anchored to the edges and defects of the MoS2 nanosheets, where S atoms act as sites for metal nuclei seeding, leading to the uniform distribution of NFO-NPs on MoS2 materials.24,35,36
![]() | ||
| Fig. 2 (a–c) SEM images of the as-synthesized materials (NFO, MoS2, and MoS2–NFO); (a′ and b′) size distribution of NFO and MoS2 samples. | ||
The Raman spectra of all synthesized samples (NFO, MoS2, and MoS2–NFO) were shown in Fig. S1.† It is evident to see NFO spectrum has 4 bands at 335, 486, 571, and 703 cm−1, as described in Fig. S1a,† matched well with earlier published reports.37,38 Fig. S1b† exhibited two characteristic peaks of MoS2 at 385 and 409 cm−1. These peaks were attributed due to the in-plane (E12g) and the out-of-plane (A1g) vibration modes, respectively. The difference between these two peaks of 24 cm−1, suggesting that the sample MoS2 has a few layers.25,39–41 For MoS2–NFO nanocomposites, the presence of characteristic peaks of both MoS2 and NFO was recorded, demonstrating the co-existence of MoS2 and NFO within the nanocomposite structure (Fig. S1c†), which is consistent with the XRD results observed.
The magnetic characteristics of synthesized samples were observed via the magnetic hysteresis (M–H) curves at room temperature. The hysteresis loops were described in Fig. 3, the value of saturation magnetization (Ms) was determined around 37.2 emu g−1 for NFO and 28.8 emu g−1 MoS2–NFO samples, while the MoS2 sample did not show a magnetic curve. The considerable decrease in Ms value when NFO NPs were combined with MoS2, is consistent with the weak magnetic properties of MoS2 sheets originating from the existence of zigzag edges within layered structure. Similarly, the Mr and the coercivity (Hc) values of these proposed samples were determined approximately 9.94 emu g−1 and 131.18 Oe for NFO, 8.6 emu g−1 and 140.79 Oe for MoS2–NFO samples, respectively. Although, the increase of magnetic property at MoS2–NFO sample was observed, it still guarantees the good magnetic response when the external magnetic field (MF) applied.
:
1)/SPE (160 μA), and MoS2–NFO (1
:
1)/SPE (155 μA) than that of bare SPE (116 μA) and even NFO/SPE (146 μA). To explain this, some kinetic parameters involving the electron transfer reaction of the redox probes were calculated and evaluated in detail. Namely, the peak-to-peak separation potential (ΔEp = Epa − Epc) from CV curves, a critical proof, reflects the limitation in electrical conductivity and charge transfer kinetics. It was determined in the order: MoS2/SPE < MoS2–NFO (2
:
1)/SPE < MoS2–NFO (1
:
1)/SPE < NFO/SPE, which is much lower than that of bare SPE for a single electron-transfer process. Clearly, the modification of the electrode surface brought out many positive improvements in conductivity and charge transfer, compared with bare SPE. Furthermore, when CV measurements were performed at various scan rates in the range from 20 to 70 mV s−1 on the proposed electrodes, the changes in response current intensity and the reversible redox peak potential were observed at all modified electrodes even in the bare SPE (Fig. S2†). In this case, the current response linearly increased in the increase of square root of the scan rate (ν1/2), corresponding to the regression equations:| Ip = 16.92ν1/2 (mV s−1) + 27.633 (R2 = 0.999) for NFO/SPE |
| Ip = 23.01ν1/2 (mV s−1) + 13.094 (R2 = 0.999) for MoS2/SPE |
Ip = 19.63ν1/2 (mV s−1) + 22.269 (R2 = 0.999) for MoS2–NFO (2 : 1)/SPE |
Ip = 20.44ν1/2 (mV s−1) + 17.227 (R2 = 0.999) for MoS2–NFO (1 : 1)/SPE |
From that, the electrochemical active surface area (EASA or A) was calculated using the Randles–Sevcik equation (25 °C) as described by equation:7,23,42,43
| Ip = (2.69 × 105)n3/2D1/2Aν1/2C |
:
1)/SPE, and 0.209 cm2 for MoS2–NFO (2
:
1)/SPE, respectively. As can see, the highest value of EASA and the lowest value of separation potential (ΔEp) were achieved at MoS2/SPE, it is in accordance with the highest value of current intensity at this electrode. This result might be since the fact that MoS2 sheets have a much larger surface area and higher electrical conductivity than NFO NPs, which facilitates an effective raise of the electron transfer and interaction in the middle of the probe molecules with the electrode surface. Further to mention, the good combination at a weight ratio of 1
:
2 between NFO and MoS2 also brought excellent enhancements for EASA and ΔEp values. As indicated in SEM images, NFO NPs were uniformly distributed onto MoS2 sheets, leading to effectively inhibiting the self-aggregation of NFO NPs and MoS2 sheets. This is beneficial for the exposure of active sites and therefore improving the conductivity and electron transfer. Additionally, the close contact between NFO NPs and MoS2 sheets suggested a strong interaction was generated at their interface. However, it needs to be noted that, at the higher weight ratio of NFO within MoS2–NFO (1
:
1) nanocomposites, the values of peak current recorded seem to have a decreasing trend, compared with that of the MoS2–NFO (2
:
1) sample. This could be followed by the excess increase of NFO NPs led to agglomeration and break of the structure of MoS2 sheets into smaller pieces. Consistency of these proposes with the values of EASA and separation potential (ΔEp) was found.
To further verify the great improvement of electrical conductivity and charge transfer kinetics arising from the modification of the electrode surface with proposed synthetic samples, electrochemical impedance spectroscopy (EIS) is considered the effective direct method to evaluate charge transfer ability onto the electrode surface.44 Fig. 4b shows Nyquist diagrams of various electrodes in a mixture solution of 0.1 M KCl solution containing 5.0 mM [Fe(CN)6]3−/4−, which confirms the difference in the electron transfer process occurring at each different electrode. In which, the electron transfer resistance (Rct) value is one of the most parameters controlling the kinetics of the electron transfer reactions of the redox probes at the electrode/electrolyte interface. This value is directly determined via the semicircle diameter in the high-frequency range. As seen, the Rct value could be estimated as approximately 487.3, 242.8, 180.9, 214.5, and 200.6 Ω for bare SPE, NFO/SPE, MoS2/SPE, MoS2–NFO (1
:
1)/SPE, and MoS2–NFO (2
:
1)/SPE, respectively. It is interesting to see that the obtained results fitted well with the CV response and separation potential (ΔEp) of all electrodes recorded. Worthy of note, the Rct value was employed to estimate the standard heterogeneous rate constant (ket) for all electrodes:23,29,45
| ket = RT/(n2F2RctACo) |
:
1)/SPE, and MoS2–NFO (2
:
1)/SPE to be around 7.1 × 10−4, 1.15 × 10−3, 1.27 × 10−3, 1.23 × 10−3, and 1.27 × 10−3, respectively. The above results manifest that benefiting from possessing high EASA, low separation potential (ΔEp) value, and small electron transfer resistance (Rct) value helped MoS2/SPE to achieve the highest ket value. More interestingly, the similar value was also observed at the MoS2–NFO (2
:
1)/SPE, demonstrating that the effective combination between MoS2 sheets and NFO NPs at the optimized ratio contributed to creating an excellent approach towards faster and easier electrons transfer reactions onto the electron surface as well as the electrode/electrolyte interface. Therefore, MoS2–NFO (2
:
1)/SPE was chosen as the optimum modified electrode for the next experiments.
:
1)/SPE were assessed through the redox reaction of CLB, proving the positive influence of surface modification with MoS2, NFO, and MoS2–NFO (2
:
1) on the sensing performance. CV measurements were traced in the presence and absence of CLB molecules at all electrodes. As mentioned in the literature, the irreversible oxidation of CLB molecules during the first anodic sweep usually occurs at around 0.8–1.0 V. At the next CV measurements, in addition to this irreversible oxidation peak, a pair of reversible redox peaks in the potential range from 0.15 to 0.3 V was recorded, reflecting the redox reaction of clenbuterol dimer molecules by an azo bond. Namely, in this case, the redox reaction of the irreversible oxidation of CLB at high potential still could be observed when the potential window of CV measurement was widened until +1.0 V (Fig. S3a†). However, this peak current intensity in the second lap decreased remarkably. In contrast, the presence of a pair of redox peaks with higher intensity at around +0.23/+0.05 V was recorded at even the first cycle as described in Fig. S3a.† To explain this phenomenon, the pre-formation of CLB dimers from hydrazobenzene derivative, which is created by the protonation of CLB molecules in solution when using the analytical standard of clenbuterol hydrochloride, is an important reason. Hence, to maintain good stability and repeatability for measurements as well as ease in observing, the redox peaks at +0.23/+0.05 V were chosen to investigate in more detail the electrochemical performance. Thus, CV measurements were carried out in the potential range from −0.3 to +0.6 V. Fig. S3b† illustrates the CV curves of bare SPE, MoS2/SPE, NFO/SPE, and MoS2–NFO (2
:
1)/SPE in pH 7.4 PBS buffer containing 50 μM CLB, respectively. The obtained results manifest that there was an increase of anodic response current and cathodic peak current at electrodes modified, particularly for MoS2–NFO (2
:
1)/SPE, which is attributed due to strong synergistic effect and excellent electrocatalytic activity within nanocomposite structure of MoS2–NFO (2
:
1). In the circumstance, CLB dimer molecules arising from formation of azo bond between hydrazobenzene derivatives attended redox reactions, corresponding to anodic/cathodic peak potential was observed at about +0.23/+0.05 V (Fig. S3a†). Also, a characteristics oxidation potential of CLB was recorded at +0.23 V while no obvious reduction peak is observed, indicating that the oxidation of CLB is irreversible. More particularly, the oxidation peak at +0.23 V was higher and clearly than that of the oxidation peak at +0.81 V. Hence, the redox peaks at +0.23/+0.05 V were chosen to investigate in more detail the electrochemical performance. In addition to the difference in current intensity, the shift of the potential position of anodic peaks at various electrodes also needs to be stressed. If at bare SPE, it was observed at 0.39 V, meanwhile, at MoS2/SPE, NFO/SPE, and MoS2–NFO (2
:
1)/SPE, the oxidation reaction occurred at lower potential values of 0.34, 0.38, and 0.37 V (Fig. S3b†). This further reflects clearly the significant improvement in electrochemical catalytic activity and electron transfer reaction kinetics at modified electrodes.
To investigate the reaction kinetics of CLB on the modified electrodes, CV measurements in pH 7.4 PBS buffer containing 50 μM CLB were carried out in the scan rate range from 20 to 70 mV s−1. The above results manifest that the anodic/cathodic peak current of all electrodes increased gradually with the increase in scan rate. The relationship between Ipa and v was illustrated in Fig. 5a′–c′, according to that it showed a high degree of linearity with linear regression equations of:
| Ip (μA) = 0.103ν (mV s−1) − 1.992 (R2 = 0.994) for bare SPE |
| Ip (μA) = 0.128ν (mV s−1) − 1.547 (R2 = 0.986) for MoS2/SPE |
| Ip (μA) = 0.167ν (mV s−1) − 2.163 (R2 = 0.983) for NFO/SPE |
Ip (μA) = 0.207ν (mV s−1) − 2.533 (R2 = 0.990) for MoS2–NFO (2 : 1)/SPE |
From that, it can be inferred that the adsorption-controlled characteristics occurred in surface-confined reactions for their electrode process. It is interesting that from the slope value of Ip vs. scan rate, the adsorption capacity (Γ) of CLB on the various electrodes was estimated at 6.9 × 10−10, 4.53 × 10−10, 7.96 × 10−10, and 4.39 × 10−10 for NFO/SPE, MoS2/SPE, MoS2–NFO (2
:
1)/SPE, and bare SPE, respectively by using equation: Ip = n2F2AΓν/4RT. Besides, the effect of scan rate on the slight shift of peak potential was studied in detail. In this case, the linear relationship between Ep and the natural logarithm of scan rate ln(ν) was described in Fig. S4,† corresponding to the regression equations as:
Ep (V) = 0.114 ln(ν) (mV s−1) − 0.282 (R2 = 0.992) for bare SPE |
Ep (V) = 0.119 ln(ν) (mV s−1) − 0.203 (R2 = 0.989) for MoS2/SPE |
Ep (V) = 0.169 ln(ν) (mV s−1) − 0.398 (R2 = 0.991) for NFO/SPE |
Ep (V) = 0.078 ln(ν) (mV s−1) − 0.123 (R2 = 0.989) for MoS2–NFO (2 : 1)/SPE |
According to the Laviron theory, the relationship between Ep and scan rate in an adsorption-controlled irreversible process can be also expressed as:46–48
| Ep = E0 + (RT/αnF)ln(RTk0/αnF) − (RT/αnF)ln(ν) |
From that, the slope value of the above lines is equal to RT/αnF, thus, the value of αn can be also determined directly. As the number of electrons transferred is equal to 1, the electron transfer coefficient value (α) of bare SPE, NFO/SPE, MoS2/SPE, and MoS2–NFO (2
:
1)/SPE was calculated to be 0.225, 0.151, 0.207, and 0.328. More importantly, the value of the electron transfer rate constant (ks) of the redox reaction of CLB at these modified electrodes was also calculated based on the equation:
ln(ks) = α ln(1 − α) + (1 − α)ln α − ln(RT/nFν) − α(1 − α)(nFΔEp/RT) |
As shown by the results, the highest value of ks was recorded at MoS2–NFO (2
:
1)/SPE of approximately 0.504 s−1, while this value only reached about 0.283, 0.331, and 0.265 s−1 at NFO/SPE, MoS2/SPE, and bare SPE, respectively. By the calculated results, although in the previous section, MoS2/SPE showed many more excellent electrochemical characteristics of electrical conductivity and the values of EASA and ket, herein, the electrochemical behaviors of CLB on the MoS2–NFO (2
:
1)/SPE exhibited more impressive improvements. Not only possessed a higher electrochemical response of CLB but the kinetic parameters related to the redox reaction of CLB showed significant enhancements. As pointed out in our previous report, CLB is a complex and bulky organic molecule, resulting in a poor flat structure when adsorbed on the electrode surface. Along with that, the CLB molecules can be protonated and self-bonded with each other, leading to the creation of a huge steric hindrance, which causes remarkable dead spaces and limitation in the adsorption ability, interaction, electron transport, and charge diffusion of CLB onto the electrode surface. More importantly, the research proved that to get higher detection efficiency for CLB, the development of unique electrodes having better charge/electron transfer and electrocatalytic activity for the redox reactions of CLB should be given priority. Maybe, in this case, MoS2–NFO (2
:
1) nanocomposite structure through the suitable and effective combination supported considerably the strong interaction and charge/electron transfer between the active material and targeted CLB molecules. Furthermore, the co-existence of MoS2 and NFO provided many active sites for better electrocatalytic activity in the redox reaction of CLB, compared with other modified electrodes.
As we know, one of the most unique properties of NFO nanomaterial is the response to magnetic fields and good electrocatalytic ability similar to other magnetic nanomaterials. In our previous research, the positive influence of external stationary MF on electrochemical behaviors of Fe3O4–carbon spheres based-electrode as well as its sensing performance towards detecting chloramphenicol was thoroughly reported.8,29,30,32,49–51 Some impact mechanisms were proposed, explaining for the enhancement in mass transfer, ionic/charge diffusion in the electrolyte solution, as well as higher absorption capacity and better electrocatalytic ability at modified electrodes. According to this inevitable trend, the utilization of MF with the aim of promoting the inherent electrochemical characteristics of MoS2–NFO (2
:
1)/SPE such as electrical conductivity, adsorption capability, and electrocatalytic activity was carried out. Also, it is expected to enhance the electrolyte's physicochemical properties, in pursuit of better response-ability and higher sensing efficiency at the modified electrode.
Indeed, under the presence of external MF, the peak current response in the CV curves of MoS2–NFO (2
:
1)/SPE increased by about 5.4% compared with the initial value when without MF. Besides, the decrease in the ΔEp value was recorded, indicating the significant enhancement of electrical conductivity and transfer kinetics in the reversible electron transfer reaction of [Fe(CN)6]3−/4− probes (Fig. S5†). More interestingly, for further investigation of the MF impacts on the sensing performance of CLB, a series of kinetic parameters involving the redox reaction of CLB onto the electrode surface was calculated. Namely, from CVs curves obtained at various scan rates in 0.1 M PBS containing 50 μM CLB under the presence of MF, it still displays a linear relationship between Ip and scan rate (ν) in the range of 20–70 mV s−1 and it can be expressed as Ip (μA) = 0.413ν (mV s−1) − 5.188 (R2 = 0.995) as Fig. S6.† Furthermore, the linear equation of Ep and logarithm of scan rate was also estimated as Ep (V) = 0.148
ln(ν) (mV s−1) − 0.278 (R2 = 0.978). According to that, ks and adsorption capacity (Γ) values of CLB achieved about 0.521 s−1 and 1.57 × 10−9, demonstrating the remarkable enhancement of electron transfer rate constant (ks) and adsorption capacity (Γ), compared with that of without MF under the same experimental condition.
To get more insight into the influence of MF on electrocatalytic activity within MoS2–NFO (2
:
1)/SPE, CA measurements were taken with and without external MF. As shown in Fig. 6a and d, the linear increase of current response for diffusion-limited electrocatalytic techniques vs. t−1/2 were found at various concentrations in both two cases. Based on Cottrell's equation:29,52,53
| I = nFAD1/2Cbπ−1/2t−1/2 |
| IC/IL = π1/2(kcatCt)1/2; |
From the direct slope values obtained in Fig. 6e and f at 20 μM CLB, the kcat were estimated around 0.0237 and 0.0329 without and with the support of MF. Consequently, it shows that the presence of MF offered many positive increases in the electrocatalytic activity of the electrode modified with MoS2–NFO (2
:
1) as expected.
The electrochemical response was remarkably affected by the pH value of the PBS buffer and accumulation time during measurement. Thus, there is necessary to optimize the experimental conditions to obtain the highest electrochemical response. In this work, DPV measurements were analyzed at various pH values, using 1 M NaOH and H3PO4 solution for controlling the pH value in the range from 3 to 11. As displayed in Fig. 7b, it shows that the peak current gradually increased with increasing pH from 3 to 5 and reached a maximum value at pH 7.4, then decreased with over-increasing pH. With the maximum current, pH 7.4 was chosen as the optimal pH value for all the subsequent electrochemical measurements. In addition, the linear shift of peak potential with the increase of pH was found as expressed by the following equation: Ep (V) = −0.034pH + 0.419 (R2 = 0.992) in Fig. 7c. Fixing on the pH 7.4, the accumulation time was measured from 20 to 200 s to find the accumulation optimization. Fig. 7d exhibits the response current achieved a maximum value at 60 s and lower at other times, which could be attributed due to the saturated adsorption state of CLB onto the electrode surface.54 Finally, the pH of 7.4 and accumulation time of 60 s was employed as the best condition parameters for further electrochemical measurement in this work.
In order to investigate the sensitivity of electrochemical response with different concentrations of CLB at MoS2–NFO/SPE, especially in the experiment without and with MF, DPV were conducted in 0.1 M PBS buffer at the optimized experimental conditions. The DPV curves with different concentrations of CLB were displayed in Fig. 8a and b, respectively. All figures display that the peak current decreased to lower values with the reduction of CLB concentration. However, in comparison to the response current without and with MF, the electrochemical response with the presence of MF was considerably higher, corresponding to the wider linear range of CLB concentration from 0.5 to 50 μM, compared with that without the presence of MF from 1 to 50 μM, particularly, for bare SPE with the limited linear range from 10 to 50 μM. As a result, the linear relationship between the current response and the concentration of CLB was recorded in both three cases: ΔIp (μA) = 0.233CClB (μM) − 0.196 without MF; ΔIp (μA) = 0.682CCLB (μM) + 0.147 with MF; and ΔIp (μA) = 0.125CClB (μM) − 0.451 for bare SPE. The limit of detection (LOD) for bare SPE, and MoS2–NFO (2
:
1)/SPE without and with MF was computed from the calibration curve of 0.878, 0.471, and 0.161 μM, respectively (Fig. 8c, d and f).
Investigating the stability, repeatability, and selectivity of the modified electrode, DPV measurements were carried out at MoS2–NFO (2
:
1)/SPE. Firstly, for evaluating the long-term stability, MoS2–NFO (2
:
1)/SPE was remained for 2 weeks at room temperature and atmosphere conditions, and then, it observed any change in the current response at the DPV curve for this electrode. As expected, only 3.4% of the initial value of the current response was reduced, exhibiting the good stability of the proposed electrode. Secondary, DPV measurements were repeated ten times in 0.1 M PBS (pH = 7.4) containing 20 μM CLB at 50 mV s−1 to assess the repeatability. The obtained result indicates that the MoS2–NFO (2
:
1)/SPE had outstanding repeatability with RSD value of 2.3%. Finally, some ions and organic molecules at 20-fold higher concentrations compared with 50 μM CLB such as Fe3+, Ni2+, Co2+, Cl−, NO3−, SO42−, Mg2+, Mn2+, ascorbic acid, glucose, urea, and nitrophenol were used as interfering substances to check the selectivity of the MoS2–NFO (2
:
1)/SPE towards the redox reactions of CLB. As pointed out, no significant influence on the current response of CLB was observed even under high concentration of interfering substances, corresponding to deviations below 4.2%. Notably, adding high concentrations of ascorbic acid owning an intense oxidation signal at about 0.17 V seems to lead to overlapping with the characteristic oxidation peak of CLB. In this case, a deconvolution tool to separate both individual signals was used. As a result, after deconvoluting this peak, the oxidation peak of CLB still displayed a high stability in response intensity as other studied interfering substances. The results recorded from stability, repeatability, and selectivity tests exhibited that MoS2–NFO (2
:
1)/SPE might be considered the best choice for the analytical application. More interestingly, in a comparison of sensing performance with other modified electrodes in the literature, it still exhibits a great enhancement in electrochemical performance toward CLB detection (Table 2). Besides, the presence of external MF is considered a promising development approach to increase performance instead of focusing on developing new synthesis methods and composites as in other reports.
To evaluate the practical application of MoS2–NFO/SPE as working electrode for detecting CLB, DPV measurements were taken in various spiked milk samples by the standard addition method. Milk concentration were added into 10-folds CLB sample. As exhibited in Table 1, it was clear that the recovery result of spiked samples was in the range from 90 to 96.32%. Meanwhile, RSD values of three times paralleled detection were obtained from 1.07 to 2.01%. These obtained results demonstrated that the proposed electrode based on MoS2–NFO was suitable accuracy and can be applied to determine the presence and concentration off CLB analysis in real matrixes.
| Samples | Spiked (μM) | Found (μM) | Recovery (%) | RSD (%) |
|---|---|---|---|---|
| Milk | 40 | 38.48 | 96.20 | 1.14 |
| 30 | 28.89 | 96.32 | 1.07 | |
| 20 | 18.19 | 90.97 | 2.01 |
| Modified electrode | Measurements | Linear range (μM) | LOD (μM) | Repeatability | Ref. |
|---|---|---|---|---|---|
| NiFe2O4–MoS2/SPE | DPV | 1–50 | 0.471 | 97.7/10 | This work |
| DPV | 0.5–50 | 0.161 | 97.7/10 | This work | |
| KVB-Nf (IP)/FCE | DPV | 0.95–14.31 | 0.75 | 99.48/10 | 55 |
| BCNO/GCE | DPV | 0.03–16 | 0.017 | — | 56 |
| MoS2–Au–PEI–hemin/GCE | DPV | 10–2000 | 1.92 | — | 57 |
| Cl/MIP/Au | DPV | 2–100 | 0.031 | — | 58 |
:
1)/SPE was the best and most promising electrode for CLB detection. Also, the presence of MF enhanced the electrochemical features of MoS2–NFO (2
:
1)/SPE and a series of kinetic parameters in the redox reaction of CLB. By optimizing the experimental conditions in terms of the pH and accumulation time, the highest electrochemical response was recorded, corresponding to the pH at 7.4 and 60 s for the accumulation time. In addition, the work also reported the added advantages such as stability, repeatability, and selectivity of the proposed electrodes. The limit of detection for MoS2–NFO (2
:
1)/SPE in the absence/present MF were 0.471 and 0.161 μM, respectively, which promises MoS2–NFO (2
:
1)/SPE will be ideally suited to develop new sensor electrodes for further effective and fast detection towards different analytical molecules.
Footnotes |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ra01136d |
| ‡ V. M. Tien and O. V. Hoang contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2023 |