Open Access Article
Esperanza
Fernández-García
a,
Uriel
Caudillo-Flores
b,
Rocío
Sayago-Carro
a,
A.
Tolosana-Moranchel
a,
Marcos
Fernández-García
*a and
Anna
Kubacka
*a
aInstituto de Catálisis y Petroleoquímica, CSIC, C/Marie Curie 2, 28049-Madrid, Spain. E-mail: mfg@icp.csic.es; ak@icp.csic.es
bCentro de Nanociencias y Nanotecnología, Universidad Nacional Autónoma de México, Ensenada 22800, Mexico
First published on 1st November 2025
Enhancing the performance of titania-based systems has emerged as a central goal to allow the light-triggered continuous production of hydrogen using renewable energy and bio-based sacrificial molecules. A cheap and widely available promoter based on magnesium is here exploited to provide a long-term stable catalytic response and maximize the formation of hydrogen. Using the International Union of Pure and Applied Chemistry (IUPAC)-recommended quantum efficiency as the parameter to measure activity, this study demonstrates an 8.2-fold increase in photocatalytic activity compared with the Pt–TiO2 reference catalyst, achieving a quantum efficiency of 3.0% under sunlight. The physicochemical study provides evidence that the increase in activity is achieved through a precise synthesis procedure, resulting in the formation of atom-dispersed Mg(II) entities. The origin of the promotion effect appears to be related to the reaction mechanism, with a limited effect from charge carrier generation or recombination. An in situ infrared study showed that the surface effects connected to the adsorption of alcohol, as well as the generation and (subsequent) evolution of bridge carbonate species, appear at the core of the enhancement in activity. The magnesium promoter, spread as single-atom entities over titania, is thus shown as a way to obtain highly active and stable photocatalytic systems for green hydrogen production.
Keywords: Single-atom promoter; Sunlight; Quantum efficiency; Mechanism; Hydrogen.
Titania is the most explored material as a photocatalyst. Its performance has been shown to be outstanding in many fields, including hydrogen production. Ways of improving titania-based materials continue to be actively investigated. The main weaknesses of titania-based catalysts relate to several physicochemical issues. Light-related ones concern limited absorption of visible light due to a 3.0–3.2 eV band gap, as well as improvable control over charge carrier recombination. Light and chemical limiting issues encountered at the reactive surface of titania are primarily related to the trapping of charge carrier species by different surface species, such as hydroxyl and vacancies, as well as the interaction of such surface radical species with the chemicals involved in the desired reaction, controlling reaction mechanism and kinetics.1–3 For hydrogen production, a key beneficial effect arises from the use of a cocatalyst, with platinum consistently delivering the best performance. Pt is known to play an active chemical role in the reaction and limits charge recombination by capturing electrons and increasing their lifetime with the help of the adequate electronic properties of the Pt–titania interface.7–9 In addition, the structural/electronic modification of titania by metals and non-metals has been extensively explored. Many metals have been tested, but particular efforts have been devoted to enhancing and controlling light absorption and charge recombination through either doping at the bulk or the use of surface species as atomic or molecular entities. The alteration of the electronic structure, particularly the valence-conduction bands and band gap energy, together with the presence of defect-related gap-localized electronic states, are commonly claimed as key factors for the improvement in activity. In addition, changes in surface connections with redox and acid–base properties are commonly pointed out as critical to obtain high activity.9–12 The resulting landscape portrays composite metal–support systems as novel top catalysts with co-catalysts and/or surface species, as well as doping species, shaping the performance of the titania-based materials. Often, such complex catalysts have specific nanostructures and/or interfaces that may be complex to maintain under reaction, particularly considering the long-term on-stream requirement for practical application.7,13–16
For cocatalyst or surface species, single-atom entities are actively sought to boost activity for hydrogen photoproduction. Nevertheless, small nanoparticles of Pt deposited on titania would show improved performance when compared with isolated and subnanometric species.17 A careful inspection of hydrogen photon production using turnover frequencies (TOF) and quantum efficiency (QE) is required to provide a clear answer to this point.18,19 The physicochemical grounds for such behavior can be strongly related to chemical effects (oxidation state of the noble metal) as well as the size-dependence of electron capture and subsequent charge recombination on platinum entities. In addition, note that the TOF and QE values for single-atom and (sub- or nanometric) cluster entities cannot, on their own, determine the average (macroscopic) values observed in a catalyst. In addition to the single-particle TOF and QE values, the corresponding macroscopic values would be determined by the population density of the different species present in a real catalyst, as well as stability issues. In this context, note that the long-term stability of the isolated platinum species on titania is dubious under (hydrogen photoproduction) reaction conditions due to agglomeration and/or leaching.9 A different situation may occur in the case of promoters with strong interaction with titania. Cationic metal-based species able to provide stable oxidic environments are typical promoters of titania.1–3,11,20 The enhancement in photoactivity has been shown to be significant in the case of (transition and rare-earth metal) single-atom entitites.21,22
Our manuscript attempts to screen a cheap and widely available promoter, such as magnesium at the surface of an anatase system, with platinum as a cocatalyst. Magnesium has been shown to provide activity as a doping agent23 or surface promoter.24 However, as shown below, the activity enhancement presented in these studies is limited. Following the IUPAC recommendations and using the quantum efficiency parameter,25 we will show an outstanding and stable promoting effect due to isolated magnesium species located on the catalyst surface. The use of a single-atom promoter is thus described as a rather useful tool to enhance the activity of well-known systems such as Pt-cocatalyst titania-based solids.
The larger entities displayed in the HR-TEM (high-resolution transmission electron microscopy) images correspond to titania nanoplatelets, showing the (101) basal plane of the anatase polymorph. This polymorph dominates the XRD (X-ray diffraction) patterns for all the PtxMg (where x is the molar content of Mg; see section 4) and reference samples (Fig. 1j). From low to high two-theta angle values in the XRD patterns of all samples, we can see the (101) peak at ca. 25.11°, the (103), (004), (102) triplet centered at ca. 37.74°, the (200) peak at 47.83°, the (105) peak at 54.04°, the (211) peak at 54.74°, the (204) peak at 62.51°, and other minor peaks at higher angles. As discussed before, all these peaks can be ascribed to the anatase phase with I41/amd space group (JCPDS card 01-084-1286).26 The primary particle size of the anatase obtained from XRD is also relatively similar for all catalysts. Table S3 includes the corresponding values, which go from ca. 10.7 nm for the PtT (platinum–titania) sample to 8.5 nm for the Pt7.5Mg solid. The presence of magnesium modestly decreases the crystallite size of the anatase nanoplatelets. The table provides evidence that Pt deposition has a relatively minor effect on anatase, as may be expected from the preparation procedure.
Textural and morphological properties of the catalysts were further investigated. Nitrogen adsorption/desorption isotherm profiles for selected samples are presented in Fig. 1k as representative examples. All the solids are mesoporous materials, owing to a characteristic H4 type loop dominated by adsorbate–solid interactions.27 BET (Brunauer–Emmett–Teller) surface area values are collected in Table S3. This parameter shows values ranging from ca. 125 to 165 m2 g−1, and increases smoothly from the PtT to the Pt7.5Mg samples. The inverse correlation between the primary particle size (crystallite size obtained from XRD) and BET area indicates that morphological differences between samples are mainly attributable to the variations in the former parameter. However, such differences are rather modest, as all samples are mesoporous materials with high surface area (over 125 m2 g−1).
Additional information about the minor components of the catalysts was obtained through the use of dark-field STEM microscopy. Fig. 2a shows a high-magnification view in which the (mostly) isolated ions are clearly detected on the anatase surface of the Pt3.75Mg sample. Very few aggregation entities of no more than 3 atoms are observed. Moreover, the EDS (X-ray energy dispersive analysis) analysis of a larger portion of the material provides evidence of the high dispersion of such entities. The presence of the (dominant) isolated single-atom entities is observed in all magnesium-containing samples using dark-field STEM. Note that such entities are absent in the STEM micrographs of the PtT reference sample (Fig. S1). The chemical nature of the single-atom species can be ascribed unequivocally by comparing the microscopic analysis of the T and 3.75Mg support solids presented in Fig. S2a–e. These entities are observed in both the bright- and dark-field microscopy images of the magnesium-containing support (Fig. 2c–e). They are located at surface positions but are absent on the T material, indicating that they can be observed only in the presence of magnesium in the support powders. Fig. S2d shows that such single-atom entities occupied surface positions out of the anatase (TiO2) crystallographic planes. These two observations strongly suggest that such entities differ chemically relative to the atoms located at anatase planes. The assignment to magnesium single-atom entities would thus be evident. EDS analysis provides evidence of the high dispersion of the atomic-size magnesium entities, achieved with our preparation method in all (magnesium-containing) PtxMg samples in the series (Fig. S3). Further evidence of the good dispersion achieved comes from a comparison with a support having the same magnesium content (3.75 mol%) and prepared using a conventional impregnation method. The differences in magnesium dispersion are evident (Fig. S2). In this context, it can be noted that the invariance observed in the position of anatase-related XRD peak(s) (Fig. 1j) is in accordance with the dominant surface position of magnesium at the anatase, with any doping effect being negligible.
Further information about the effect of magnesium on physicochemical properties of the solids was obtained through the measurement of the optoelectronic properties with the help of UV-visible and photoluminescence spectroscopies. UV-visible spectra (Fig. 2c) are dominated by the main (by weight) anatase component. An S-type shape is observed, demonstrating the semiconductor nature of the anatase. Anatase is, as mentioned earlier, an indirect gap semiconductor,28 and the band gap values of the samples obtained are also reported in Table S3. A roughly constant value of 3.1 to 3.3 eV is obtained for all samples, a value characteristic of the anatase polymorph.11 Additionally, a flat, ill-defined tail extending throughout the visible region (up to ca. 550 nm) of the spectra is also detected. This is commonly attributed to lattice vacancies, which seem to grow with the Mg content.11,29 The photoluminescence spectra allow analysis of the defect states. Under UV excitation, defect-related states (particularly anion-related defects in the case of anatase) contribute to anatase de-excitation. Anatase-based systems normally present two well-differentiated de-excitation processes, called green and red, as shown in Fig. 2d. These bands are connected with band-to-defect-related electronic transitions, the green one sampling defects near the conduction band and the red one near the valence band.30,31 The photoluminescence signal shows a consistent decrease in intensity relative to the PtT reference. This happens irrespective of the excitation wavelength. This fact strongly suggests that the tail observed in the UV-visible spectra would be related to near-band, edge-type localized electronic states.32,33 In this case, surface states associated with magnesium in strong interaction with anatase create small distortions in the density of states at the edge of the conduction/valence bands. Although the corresponding density of states is rather small, these electronic states allow light absorption in the visible range. The study of the optoelectronic properties was carried out using linear potential sweep photoresponse experiments (Fig. S4). They show that, when the light was off, no current was detected. Conversely, when the photoelectrodes were irradiated, for most of the catalysts, the photoresponse density increased almost linearly upon increasing the applied potentials from 0 to 0.8 V vs. Ag/AgCl. However, exponential growth was noted at higher potential. Such positive current densities are ascribed to the oxygen evolution reaction (OER) under irradiation and can be used to evaluate their activity. The Pt5Mg photocatalysts yielded the greatest photoresponse density (65 μA cm−2 at 0.75 V vs. Ag/AgCl), followed by Pt3.75Mg, Pt2.5Mg and Pt1Mg, which provided similar values (around 51 μA cm−2 at 0.75 V vs. Ag/AgCl). Regardless of the Mg concentration, all the photocatalysts performed better than PtT at potentials above 0.25 V vs. Ag/AgCl. These results confirm the improved charge separation displayed in the presence of magnesium, which entails longer electron lifetimes. The decrease in photoresponse observed for the photocatalyst with the highest Mg concentration (33 μA cm−2 at 0.75 V vs. Ag/AgCl), Pt7.5Mg, could be due to changes in the above-detected defect-related states that lead to a slow electron–hole separation rate.34,35
XPS (X-ray photoelectron spectroscopy) was used to further analyze the electronic effects connected with the presence of the defects detected in the UV-vis and photoluminescence studies. The O1s peak contains information about several oxygen species, e.g., lattice oxygen, defects and surface species, mainly OH and adsorbed H2O.36,37 Fig. S5 schematically shows the binding energy regions of these three species using the PtT sample. In the figure, the overlap between the last two mentioned oxygen-containing species is highlighted (in color). In any case, the modest growth of the intensity in the 531–532 eV region is in line with the above results. A similar conclusion can be obtained by detailed analysis of the valence band of the solids and the electronic states observed above its edge (Fig. S5). Therefore, certain mild growth of defects with the magnesium content is observed, although such growth does not display simple behavior or correlation with magnesium content. Moreover, analysis of the valence band evidences the lack of differences in the top-edge energy between the samples (Fig. S5). The constant band gap value on the samples (Table S3) indicates the relatively limited changes in valence and conduction band positions (particularly for samples with an Mg molar content below or equal to 5%) throughout the series of samples studied.
In summary, the analysis of defect structures using XPS, photoluminescence, and photoresponse measurements indicates that magnesium promotes the generation of (mainly) oxygen-associated defect states in the PtxMg samples, although the extent of these defects does not show an obvious correlation with magnesium content. We would like to remark that the observed decrease in photoluminescence intensity in the presence of magnesium would promote the number of charge carrier species and the charge carrier lifetime. As a result, the probability of a charge carrier reaching the surface and its involvement in the chemical steps of photocatalytic processes both increase.30,38 Apart from that, rather limited changes are observed in other electronic properties, particularly the band-edge position of the valence and conduction bands.
The physicochemical characterization of the platinum- and magnesium-containing components was completed using XPS analysis. First, we note that the commonly scanned Pt 4f is distorted by the Ti plasmon peak in the presence of anatase.36,39 For this reason, we also scanned the Pt 4d peak. As shown in Fig. S6, the Pt 4f7/2 and Pt 4d5/2 XPS signals display binding energies at 70.4 and 313.8 eV, respectively. They are both characteristic of metallic platinum species.36 A key point is that the signal (intensity and binding energy) is essentially invariant throughout the series of samples. In agreement with the microscopic study, the average particle sizes of the Pt(0) nanoparticles present in the samples of the series do not show significant differences. The Mg 1s XPS peak was also recorded for our samples (Fig. S7). The Mg 2p XPS peak has limited utility due to its strong overlap with Pt 5p3/2 XPS peaks.36 The limited occupancy of the 1s orbital (two electrons), as well as the limited absorption coefficient for single-atom magnesium entities, would make the signal relatively weak, yet, as expected, the intensity grows with the magnesium content of the material, as was previously discussed in light of other techniques (Fig. S7). In addition, the 1 s Mg XPS peak displays a constant binding energy throughout the series of ca. 1304.2 eV. This binding energy is characteristic of Mg(II) species in oxidic environments.36
Finally, the acidity and basicity of the catalysts were studied using thermo-programmed desorption experiments with NH3 and CO2 as probe molecules, respectively. Fig. S8 shows the results of the aforementioned tests. The adsorption capability of the solids is customarily analyzed in terms of the low, medium and high adsorption strength fractions. This physicochemical parameter, adsorption strength, is directly connected to the desorption temperature of the probe molecule from the catalyst surface.40,41 The two upper files of Fig. S8 (panels a–d) show representative examples of such analysis for selected catalysts. The bottom panel (Fig. S8e) of this figure provides a comparison of the adsorption capability of the samples. A mild increase in basicity is observed in the presence of magnesium. Magnesium significantly decreases the acidity of the surface by decreasing the population of the medium-strength acid sites and increasing that of low-strength acid sites, which then become dominant.
:
water ratio, and the illumination intensity.42–44 The response of our catalysts was analyzed using a Box–Behnken factorial design.45Fig. 3 displays the results of this study for the PtT and Pt3.75Mg samples, while Fig. S9 shows the results for the Pt5Mg catalyst. To study the response to the abovementioned variables, Pareto plots (Fig. S10) were utilized to visualize the catalytic response of the solids, which was modelled using linear, quadratic and crossed terms between the three factors.46 Pareto charts of standardized effects provide graphical evidence of the statistically significant parameters, that is, those that are above the established threshold. For a parameter to be statistically significant, the null hypothesis of the parameter coefficient being equal to zero is tested by comparing the calculated ANOVA p-value with a significance test level here set at α = 0.05 (95% probability). If the p-value is less than α, the hypothesis that the coefficient is equal to zero is rejected, and it is deemed to be statistically significant. In Fig. S10, the length of the plotted bars is a graphical representation of the weight of the parameters.
The Pareto plots provide evidence of the profound effect of magnesium on photocatalytic behavior (Fig. S10). The response of the PtT sample is essentially sensitive to irradiation in the ranges studied (Fig. 3). The irradiation level triggers a response with a rough power dependence of 0.5 of the intensity at the reactor (
measured as described in the SI section, eqn (2)). This behavior has been observed previously and was discussed in detail in kinetic studies of hydrogen photoproduction.43 The optimum methanol
:
water ratio is close to a CH3OH
:
H2O 50
:
50 ratio for all samples. The response to different methanol
:
water mixtures was extensively studied previously, showing increasing behavior for methanol concentrations up to ca. 30% and steadier behavior for higher concentrations of alcohol. The optimum of 50
:
50 or methanol-rich mixtures is typical of platinum-promoted anatase systems.20,47 For the catalyst concentration, the most important effect is the significantly lower quantity required to optimize the response in the presence of magnesium at the catalyst composition. The optimum catalyst concentration changes from 0.27 mg mL−1 for the PtT sample to 0.12 mg mL−1 for the Pt3.75Mg sample (Fig. 3). The minimum quantity of magnesium included in the catalyst formulation (Pt1Mg) has a strong effect, with an optimum concentration of 0.17 mg mL−1. The result of the optimization is that magnesium is able to enhance the reaction rate by ca. 10.4 times (Pt3.75Mg vs. PtT). The strong catalytic effect of atom-dispersed magnesium entities is thus evident. The combined effect of platinum and magnesium can also be noted, taking into account that the 3.75Mg support presents rather low activity, nearly 23 times lower than that of the Pt3.75Mg sample. Meanwhile, carbon dioxide was the only gas-phase molecule detected along with hydrogen in the experiments. This was also observed in previous contributions.8,18,48 The CO2 production rates are presented in Table S4.
To further study the promotion effect of atom-dispersed magnesium, we analyzed the quantum efficiency parameter. Quantum efficiency describes the performance of the catalyst per unit photon (Einstein) absorbed by the powder under reaction conditions. It is the parameter that the IUPAC (International Union of Pure and Applied Chemistry) recommends to compare the activity of photocatalysts.25,49 A comparison of the activity performance of our samples and benchmark materials is presented in Table S5.
To obtain quantum efficiency values, Fig. 4 displays the relevant optical properties of the catalyst suspension for values of the reaction medium (methanol-to-water ratio) and illumination conditions rendering optimum catalytic response (Fig. S11, Table S6). Note that this takes place with a single difference between the (reaction) operation variables, the optimum catalyst concentration around which the catalytic activity was studied (Table S6). The optical variables relevant for analyzing activity for a suspended catalyst (liquid phase) are described in eqn (1) and (2) (section 4.3). For representative samples, the spectral extinction coefficient (βλ), spectral absorption coefficient (κλ), and the spectral scattering coefficient (σλ) are presented in Fig. 4a and b for the UV-visible range. The corresponding local volumetric rate of the photon absorption (Ea) parameter over the (z, r) plane of a (cylindrical) reactor volume is shown in Fig. 4c and d. The entire reactor volume is obtained by repeating this plane by rotation around the central axis of the reactor (Fig. S12b). The effect of magnesium on the relevant optical properties of the catalyst suspension becomes evident in the radial-averaged Ea,ν profiles displayed in Fig. S13. The step decrease in the PtT signal is likely a critical effect for optimizing the solid–light interaction under reaction conditions. As a result of the strong differences in optical properties and light intensity at the reactor, the response of the catalyst should be compared at optimum conditions for all samples, as previously indicated.43
The reaction rates and corresponding quantum efficiency values for the catalysts of the series under optimum conditions (maximizing the catalytic response) are presented in Fig. 4e. Both parameters show relatively similar behavior throughout the series of samples. The optimum activity seems to be located for a magnesium concentration of 3.75 to 5 mol%. As mentioned, a comparison with previously reported reaction rates of magnesium-promoted systems is shown in Table S5 (entries 1 and 2). Although previous work uses different reaction conditions, making a clear assessment difficult, the rates expressed per gram of catalyst are significantly lower than those presented here. One of the studies reported the photonic yield for single-line excitation (350 nm) but did not report the corresponding solar illumination (AM 1.5G).24 Considering the information presented in the above mentioned contribution, it would be below 2%. Comparison with our best sample (Table S5; Pt3.75Mg), rendering a near ca. 50% higher quantum efficiency, provides evidence for the strong promotion effect of magnesium, as measured by both the reaction rate and the quantum efficiency. A general comparison with literature reports for titania-based catalysts is also presented in Table S5. Again, differences in measurement conditions do not make it easy to compare results. Nevertheless, reaction rates of our samples are among the highest (Table S5, entries 1–8). Comparison using the (true) quantum efficiency, the only parameter allowing quantitative analysis, can only be carried out with a very few systems, although it also favors our systems (Table S5, entries 7 and 8). Furthermore, we would like to stress the fact that, according to the quantum efficiency parameter, when using the Pt3.75Mg sample, the PtT reference activity is improved by 3.1/8.2 times under UV/sunlight (AM 1.5G). Moreover, using the TOF parameter (calculated with the dispersion values presented in Table S2), the Pt3.75Mg sample displays a value of 2790 h−1, a multiple of ca. 10.6 times the value of the PtT reference.
The results presented in the previous subsection (2.2) were able to show the similar electronic properties of the solids. Analysis of the optoelectronic properties (photoluminescence spectra, Fig. 2d, and photoresponse results, Fig. S4) provides evidence that charge carrier effects do not determine or control optimization of the photoactivity in our samples. In particular, rather similar structural/electronic properties were observed for samples with a magnesium molar content between 1 and 5%. Despite the positive role played by Mg in decreasing charge recombination and increasing electron transport capability under illumination, no obvious correlation is observed between catalytic performance (quantum efficiency; Fig. 4e) and photoluminescence/photoresponse intensity (Fig. 2d and S4) throughout the series of samples. In parallel, the surface properties of the solids were analyzed using TPD and two probe molecules (CO2 and NH3). This study shows that the presence of magnesium alters the acidity of the surface (Fig. S8d).
To interpret the effects of magnesium on activity triggered by the modification of the surface properties, we carried out in situ infrared experiments in the dark and under illumination conditions. Fig. 5c and d display results for the PtT and Mg3.75Mg samples, and Fig. S15a for the Pt5Mg sample. For the PtT reference, the adsorption of the reaction mixture in the dark shows a displacement of the water (negative band corresponding to the bending mode at ca. 1640 cm−1) by carbon-containing species. These species generate only very weak and ill-defined bands. Under illumination, a broad and prominent band appears at ca. 1583 cm−1 with shoulders at ca. 1496 and (a rather weak one at) 1685 cm−1 (Fig. 5c). These bands can be attributed to carbonates and carboxylates at the anatase surface.18,50–52 Clear differences can be visualized when comparing the in situ infrared results of the PtT reference and two active single-atom-promoted magnesium samples (Pt3.75Mg, Fig. 5d, and Pt5Mg, Fig. S15a). Magnesium-promoted samples present several bands in the dark. A band at ca. 1035 cm−1 is observed and assigned to the C–O stretching of methoxy species.50,53 A first difference thus comes directly from the promoted interaction with the sacrificial molecule, the alcohol (Fig. S15b). Other bands are observed at 1457–1458, 1568–1579, and 2020 cm−1. The first two bands can be assigned to bridge formate species, and the last corresponds to carbonyl species adsorbed over Pt nanoparticles.18,50–52 Differences between active samples would concern mainly the lower adsorption capability of methanol for the Pt5Mg sample (Fig. S15b), but the higher capability of formation of bridge formate species with respect to Pt3.75Mg (Fig. S15c). Similar behavior is observed for PtxMg (x = 3.75, 5) in the C
O stretching region (2020 cm−1; Fig. S15d), Pt5Mg showing higher surface coverage values for (carboxylate-type and) CO species.
The IR study demonstrates that the presence of atom-dispersed magnesium entities has a strong effect on the methanol coverage of the anatase surface but also plays a relevant role in the reaction mechanism and kinetics. The presence of magnesium favors the attack of the hole-related species (h+/OH˙−) on the surface-adsorbed methanol molecule. This mainly occurs through a step-like mechanism with the potential formation of several (oxidized) carbon-containing intermediates, such as aldehyde-type, acid-type precursors and, finally, carbon oxide molecules.54,55 In our case, it renders bridge-carboxylate as the main surface species (CH3OH + H2O + 4 h+ → CHOOH + 4H+). Note that this generates protons from both the alcohol and water molecules. Although water can play a role (mainly through hydroxyl-type radical species) in all the above mentioned oxidation steps, the formation of carboxylate species appears as the first step (in the step-type oxidative mechanism of the alcohol), where water is consumed. Such consumption does not take place, for example, in the generation of aldehyde-type precursor species. In any case, carboxylate-type species and maybe other minor species appear to suffer decarbonylation-type reactions generating CO and more protons (CHOOH → CO + OH− + H+).18,42,48 Finally, in the case of the magnesium-containing active samples, CO at Pt surfaces is transformed through the reverse water-gas-shift reaction (CO + H2O ↔ H2 + CO2).18,50,52 The latter renders CO2, the single carbon-containing molecule detected in the gas phase, as observed previously in other studies.8,18,48 Note thus that the carboxylate-type species do open a reaction pathway out of the step-like mechanism. Evidence of the key role of the carbonyl intermediate to promote activity can be obtained from IR results using a physical mixture between the PtT sample and the 3.75Mg support (Fig. S16). The absence of the above mentioned carbonyl species can be noted, indicating that both magnesium and platinum components of the active PtxMg catalysts are required to rapidly produce the carboxylate species.
The radar plot presented in Fig. 6a summarizes the most relevant results to interpret activity on a physical basis, and Fig. 6b provides a schematic representation of such properties. After the previous discussion, Fig. 6a compares the activity of the samples with the acidity–basicity “strength” of the surface (as measured using TPD results), the surface concentration of methanol and CO (derived from IR results; note that carboxylates and CO species demonstrate rather similar behavior for each active PtxMg sample of the series; Fig. S15) as well as the CO2 production rates. The magnesium promotion effect is maximized by the enhancement of: i) the adsorption capability of the surface for the sacrificial molecule, as a consequence of the decreased acidity of the surface, and ii) the subsequent reaction steps related to the hole attack on the molecule, decarbonylation and the water-gas-shift reaction. Comparison of the two best samples (Pt3.75Mg and Pt5Mg) would indicate that the population of the anatase surface by single-atom magnesium entities reaches an optimum (measured using the quantum efficiency parameter) for the Pt3.75Mg case, where the transformation of methanol to bridge carbonate is followed by quick evolution of this last surface species, leading to carbon monoxide (and dioxide) species (Fig. 6). Above that optimum (Pt3.75Mg), the Pt5Mg sample would show a decrease in the interaction with methanol, disfavoring its adsorption, and the transformation of the bridge-bonded carboxylate and CO species appears to be somewhat slower, facilitating the growth of their surface population (Fig. 6a). As previously mentioned, in all the above discussed steps, hydrogen ions are co-generated. At the cocatalyst (platinum) surface, these ions and electrons are efficiently combined to maximize the hydrogen yield (Fig. 6a and b). The role of platinum in such a step and the water-gas-shift reaction would be relatively similar in all active samples. This could be a consequence of the rather similar primary particle size and dispersion (Fig. 1, Table S2), and interaction with the magnesium-promoted support. Note that the facile decomposition of carboxylate species and the concomitant production of carbonyl-type species both require the participation of magnesium and platinum species at the surface of PtxMg samples. This is schematically shown in Fig. 6b. The mechanism of the interaction between platinum and magnesium is likely to involve effects on the surface diffusion of intermediate species. In any case, Fig. S16 shows the infrared results for a physical mixture between the PtT reference and the 3.75Mg support. The species detected, as well as their evolution under reaction, display strong similarities (obviously, the signal is weaker) with the PtT reference sample, where the carboxylate-type species appear to show restricted evolution, limiting activity.
A content of Mg between 3.75 and 5 mol% optimizes activity and triggers stability under long-term operating conditions. The promoting effect is here measured using a full experimental design (methanol-to-water, catalyst concentration, and illumination intensity) and comparing the reaction rates and, more importantly, the quantum efficiency values rendered by the samples. The photocatalytic activity, expressed in terms of quantum efficiency, increased 8.2-fold relative to the Pt–TiO2 reference under sunlight. This appears to be the maximum value achieved so far, to the best of our knowledge, using magnesium as a promoter. The presence of atom-dispersed magnesium species favored the control over charge carrier recombination and handling, yet the photoluminescence and photoresponse experiments showed limited influence on maximizing the activity. In contrast, the in situ infrared experiments rationalize the promotion of catalytic activity. The atom-dispersed promotion has a significant influence on both the adsorption of the sacrificial molecule as well as its evolution on the anatase surface to generate bridge formate species via hole attack. This carbon-containing species appears to decarbonylate and generate CO, which, in turn, is transformed with the help of the platinum co-catalysts through the water-gas-shift reaction. As a result, a cheap and widely available single-atom magnesium promoter appears to be an economically and environmentally respectful way to obtain hydrogen from renewable energy and bio-based carbon-based sources.
:
3) was added dropwise to the final microemulsion. The microemulsion utilized water/(Ti + Mg) and water/surfactant molar ratios of 18 and 110, respectively. The hydrolysis of the titania precursor initially produces molecular entities with unbalanced electrostatic charge, enabling their easy interaction with magnesium ions.18 After overnight stirring, the suspension was centrifuged, decanted, rinsed (methanol and Milli-Q water), and dried in a furnace at 100 °C overnight. Finally, the powders were thermally treated at 450 °C for 2 h.
The platinum cocatalyst (1 wt% with respect to the support) was introduced in the catalyst composition using a chemical deposition method. An H2PtCl6 (Sigma-Aldrich) compound was utilized as a precursor. In the first step, the calcined support was introduced into the water and sonicated for 30 min under a nitrogen atmosphere. The platinum precursor was then added to the suspension. Finally, the NaBH4 was used as a reducing agent to convert the noble metal to its zero-valent state. The Pt
:
NaBH4 molar ratio utilized was 1
:
5.18 The resulting suspension was sonicated for 15 minutes, and the resulting solid was recovered by centrifugation, washed several times with deionized water, and finally dried overnight at 80 °C. The synthesized powders were labeled Pt/xMg, where x indicates the molar amount of magnesium with respect to the Ti cation present in each solid. Thus, x was essayed from 0.5 (0.5
:
99.5Mg
:
Ti) to 7.5 (7.5
:
92.5Mg
:
Ti). A Pt–titania (PtT) reference system was also synthesized.
Diffuse reflectance infrared spectroscopy (DRIFTS) was utilized to measure the catalyst response to the reaction environment. The apparatus is a Bruker Vertex 80 FTIR spectrometer using an MCT detector and running under OPUS/IR software. A water-to-methanol mixture (optimum of the factorial design described in section 2.2) was injected into an Ar stream (10 mL min−1) and contacted with the catalyst in a reaction cell (HVC, Harrick Scientific) located in a praying mantis DRIFTS accessory (Harrick Scientific). The illumination source is the same as that used in the reaction experiments (see below). The DRIFT signal was accumulated for ca. 1.5 s for a total of 10 scans over the 4000–600 cm−1 range. The background is taken before the reaction mixture enters the reaction chamber. Contact with the reaction mixture takes place under dark conditions and is continuously scanned until stability of the IR signal of the absorbed species is achieved. After the light is switched on, the IR signal is also monitored until stability is reached.
Thermo-programmed desorption experiments were carried out using a U-shaped home-made reactor coupled with a thermal conductivity detector (TCD). CO2 and NH3 molecules were used to analyze surface basicity and acidity, respectively. Samples were subjected to a stream of the corresponding gas at 50 °C, subsequently subjected to a purge with nitrogen until a stable TCD signal was achieved and then subjected to a temperature ramp at a rate of 10 °C min−1.
:
water (tested from 30
:
70 to 70
:
30 v/v) was used to produce hydrogen gas. The reactor has a volume of 80 mL, and the suspension occupies 40 mL. The hydrogen gas was evacuated continuously from the reaction using an Ar stream (10 mL min−1). The Ar stream was stabilized under dark conditions.
Two experiments, under UV (280–400 nm) and visible (400–680 nm) light, were carried out using an Xe 500 W arc lamp coupled with dichroic and IR filters (Quantum LOT). The optimal reaction conditions to carry out the reaction were analyzed using a Box–Behnken factorial design (Table S5). The gas–liquid reactor and experimental procedures to optimize the catalyst concentration, methanol
:
water, and the illumination intensity ratio are described in the SI section and are based on previous work.7,18 Hydrogen production was obtained in continuous mode (Fig. S1) and measured using mass spectrometry (Omnistar 200; Pfeiffer). Values for the hydrogen production rate and the quantum efficiency parameters were obtained following IUPAC-recommended procedures.25Eqn (1) shows the calculation of the quantum efficiency. It utilizes the reaction rate (r) and the local volumetric rate of photon absorption (Ea). Both parameters correspond to average values (subscript A) obtained over the entire volume of the reactor.
![]() | (1) |
). With this information, the radiative transfer equation (RTE) (eqn (2)) was solved in our reactor.![]() | (2) |
) was calculated. Finally, the Ea parameter can be obtained:
. Full details of the calculation of the parameters described in this subsection can be found in previous work and are summarized in the SI (section Liquid Phase Reactor: Local volumetric rate of photon absorption calculation).7,18,49
Supplementary information is available. See DOI: https://doi.org/10.1039/d5im00219b.
| This journal is © Institute of Process Engineering of CAS 2026 |