Gang
Wang
a,
Hao
Chi
a,
Yang
Feng
b,
Jie
Fan
a,
Nanping
Deng
*a,
Weimin
Kang
*a and
Bowen
Cheng
*c
aState Key Laboratory of Separation Membranes and Membrane Processes, School of Textile Science and Engineering, Tiangong University, Tianjin, 300387, PR China. E-mail: dengnanping@tiangong.edu.cn; kangweimin@tiangong.edu.cn
bState Key Laboratory of Advanced Chemical Power Sources, College of Chemistry, Nankai University, Tianjin 300071, PR China
cSchool of Material Science and Engineering, Tiangong University, Tianjin 300387, PR China. E-mail: bowen15@tiangong.edu.cn
First published on 22nd June 2024
Designing efficient, stable and low-cost bifunctional oxygen electrocatalysts for metal air batteries is crucial and challenging. The study reports a simple and controllable synthesis strategy of polycrystalline high entropy fluoride modified porous carbon nanofibers ((MnNiCuCoZn)F2-PCNFs) for bifunctional oxygen electrocatalysis. The (MnNiCuCoZn)F2-PCNFs feature continuous and facilitated pathways and a porous structure for electron transportation and mass diffusion, providing an ideal environment for electrocatalytic reactions. The multi-principal element characteristic of high-entropy fluoride also offers a wealth of active sites to enhance the oxygen reduction reaction (ORR) and oxygen evolution reaction (OER). The zinc component leads to the transformation of high-entropy fluoride nanoparticles from single-crystal to polycrystalline, thereby effectively increasing the likelihood of exposing electrocatalytically active sites. Therefore, the prepared (MnNiCuCoZn)F2-PCNFs exhibit superior electrocatalytic performance for the ORR (E1/2 = 0.852 V) and OER (η10 = 310 mV). The assembled (MnNiCuCoZn)F2-PCNF-based ZABs achieve a high peak power density of 206 mW cm−2 and stable operation for more than 400 h. The corresponding DFT calculations further reveal that the zinc component in (MnNiCuCoZn)F2-PCNFs can lead to a continuous distribution of the density of electronic states at the Fermi level, thereby facilitating electron transfer. It can also significantly optimize the energy layout of reaction intermediates, substantially reducing the energy barriers for the ORR and OER (from 1.80 eV to 1.03 eV for the ORR and from 1.35 eV to 0.73 eV for the OER). The study proposes a “polycrystalline transition” that paves a novel pathway for the structural design of high-entropy nanoparticles and holds significant importance for the development of advanced multifunctional electrocatalysts.
For a long time, in the field of electrocatalysts and ZAB application, the mainstream ideas have been to achieve high catalytic activity of materials through using various modification methods such as heteroatom doping,19 single atom modification,20 oxygen vacancy engineering,21etc. The emerging field of high-entropy materials (HEMs) brings new ideas and attempts to understand what material properties will occur at the limit of extreme disorder.22 In HEMs, various elements are mixed in roughly equal-atomic proportions, and disorder is no longer a weak perturbation but a dominant effect. Currently, four main effects of HEMs have been widely accepted, namely the high entropy effect, lattice distortion, sluggish diffusion and the cocktail effect.23 Specifically, the advantages corresponding to these effects are as follows: (i) the high entropy effect reflects the main contribution of mixing entropy to the formation of a homogeneous phase and improves the thermodynamic stability of the catalyst.24 (ii) Lattice distortion is due to the size differences between various atoms in HEMs causing the lattice points to deviate from the ideal position.25 (iii) The sluggish diffusion effect means that lattice distortion leads to an increase in the diffusion activation energy of atoms in the lattice, thereby reducing the effective diffusion rate of atoms and improving the dynamic stability of the catalyst.26 (iv) The “cocktail” effect refers to a synergistic effect brought about by the interaction between various elements, which can construct a more ideal electronic structure to achieve efficient catalysis.27 All of these factors can provide HEMs with versatile merits, thus making them widely used in electrocatalytic systems.28–30 As everyone knows, HEMs can be classified into high-entropy alloys (HEAs), which exist only as metal atoms, and high-entropy compounds (HECs), which exist in the form of compounds. The structure formed by the interaction of multiple elements on the surface of high-entropy materials creates a wide range of potential atomic configurations, which leads to high-entropy alloys demonstrating that enhanced oxygen catalytic performance can be realized.31 For example, Chen et al.32 employed a metallurgical approach to develop a (CrFeCoNi)97O3 bulk O-HEA, demonstrating exceptional electrocatalytic performance for the OER. The coordination of some anions to form HECs is an effective method to further improve the oxygen catalytic performance.33,34 Furthermore, Dai et al.35 also synthesized a high-entropy fluoride that can exhibit an ultra-low overpotential of 314 mV at 10 mA cm−2 for the OER. Due to its highest electronegativity (4.0), fluorine can modulate the electronic properties of the prepared catalyst through a strong charge delocalization effect, thus reducing charge transfer resistance, facilitating fast mass transfer and enhancing oxygen catalysis.36
In addition to the above methods being applied to improve oxygen redox performance, various crystal structure design strategies can be employed to enhance the activity of electrocatalysts such as crystal structure porosification,37 specific crystal facets on single crystals,38 polycrystalline structures synthesis and so on.39 For example, Dette et al. designed and prepared polycrystalline hydroxides of Fe/Co/Ni with high roughness which could significantly increase the surface roughness when compared with their single-crystal counterparts, thereby increasing the number of active sites for OER catalysis.40 Consequently, transferring the polycrystalline transformation strategy to the field of high-entropy materials holds promise for further enhancing their oxygen electrocatalytic activity. In various practical strategies, the atomic rearrangement of crystals with increasing temperature may lead to the transformation from single-crystal to polycrystalline, which is a feasible method among many methods.41 Inspired by this, introducing zinc with a low melting point into high-entropy materials could result in atomic rearrangement during the calcination process.42 This may induce the polycrystalline transformation of high-entropy materials, thus increasing the number of electrocatalytically active sites. However, the zinc-containing high-entropy alloys reported so far have not shown this phenomenon, which may be due to the over-rapid diffusion of zinc in metal particles.43–45 Therefore, introducing anions to coordinate with metals to enhance the retardation of diffusion in high-entropy materials, and inducing polycrystalline transformation through zinc atomic rearrangement at high temperatures, is a feasible approach. However, no relevant studies have been reported so far.
In this work, a series of middle-high entropy fluoride modified porous carbon nanofibers ((MnNiCu)F2-PCNFs, (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCuCoZn)F2-PCNFs) were successfully designed and prepared based on electrostatic spinning and calcination for the ORR and OER. The obtained (MnNiCuCoZn)F2-PCNFs with the continuous conductive channels and porous structure, provide an ideal environment for electrocatalytic reactions. The multi-principal element characteristic of high-entropy materials also offers enough active sites, effectively accelerating the electrocatalytic processes of the ORR and OER. Zn transforms high entropy fluoride crystals from single crystal to polycrystalline, which could greatly enhance the contact areas between high entropy fluoride crystals and the liquid electrolyte for more active sites. Therefore, (MnNiCuCoZn)F2-PCNFs exhibit excellent electrocatalytic activity for the ORR (E1/2 = 0.852 V vs. RHE) and OER (η10 = 310 mV, η10 = Ej=10 − 1.23 V vs. RHE). The assembled ZABs using the prepared electrocatalysts exhibit a peak power density of 206 mW cm−2, a characteristic capacity of 760 mA h g−1, and a stable charge–discharge cycle capability of more than 400 h. Moreover, the related simulation calculations based on density functional theory have revealed that zinc can also modulate the density of electronic states to facilitate rapid electron transfer, and optimize the energy distribution of the reaction transition state to concurrently lower the energy barriers of both the ORR and OER.
Fig. 1 Schematic diagram of the preparation of high entropy fluoride modified porous carbon nanofibers. |
The high-resolution transmission electron micrograph (HR-TEM) of (MnNiCu)F2-PCNFs (Fig. 2a2) can be identified using clear crystal plane diffraction fringes with a spacing of 0.31 nm, so it is speculated that they are the (101) crystal plane of the obtained M/HEFs. The prepared (MnNiCuCo)F2-PCNFs were identified with an interplanar spacing of 0.23 nm, which was speculated to be the (111) crystal plane of the obtained M/HEFs. And in the obtained (MnNiCuZn)F2-PCNFs, two different groups of crystal plane spacings can be identified, which are speculated to be the (101) crystal plane and (211) crystal plane, both of which are belonging to M/HEFs. Among them, the exposed part of the (101) crystal plane has a relatively regular shape. But the divided (211) crystal planes are dispersed throughout the M/HEF, and part of it is even surrounded by the formed (101) crystal plane. The fluoride in the formed (MnNiCuCoZn)F2-PCNFs also exhibits a similar polycrystalline structure in which multiple crystal planes co-exist and stack on each other. However, the crystallographic faces in the prepared (MnNiCuZn)F2P-CNF can be completely surrounded by other crystallographic faces (higher degree of disorder), and the crystallographic faces in the (MnNiCuCoZn)F2-PCNF are more ordered and aggregated when compared with other M/HEF. In addition, the corresponding selected area electron diffraction (SAED) was performed to further prove whether the crystals were polycrystalline (Fig. S1†). The electron diffraction patterns without rotational symmetry indicate that the single-crystal grain structure of (MnNiCu)F2-PCNFs and (MnNiCuCo)F2-PCNFs can be formed (Fig. S1a and b†).38 The clearly rotationally symmetric electron diffraction patterns demonstrate that the polycrystalline state of (MnNiCuZn)F2-PCNFs and (MnNiCuCoZn)F2-PCNFs can be realized (Fig. S1a and b†).54–56 For exploring the reasons for the formation of the polycrystalline structure, the melting and boiling points of various related substances have been compiled according to the Lange's Handbook of Chemistry42 as shown in Table S1†. The melting and boiling points of each metal fluoride are lower than the corresponding carbonization temperature. The carbonization temperature is higher than the melting point of zinc metal but lower than the melting point of other metals except zinc. The carbonization temperature even approaches the boiling point of zinc metal. Since a large amount of reducing gases such as carbon monoxide will be produced during the carbonization process, they may compete with the fluorine in the fluoride, which may cause the fluoride to be reduced to a metallic state, and then melt or even vaporize, causing internal stress changes, thereby greatly inducing crystal rupture. The formation process may be the reason why the fluoride in the prepared (MnNiCuZn)F2-PCNFs, and the (MnNiCuCoZn)F2-PCNFs can be identified as polycrystals with multiple coexisting crystal faces and stacked on each other. But the fluoride particles in the (MnNiCu)F2-PCNFs and the (MnNiCuCo)F2-PCNFs both present independent crystals with a single crystal plane. The increased exposed surface of particles due to transformation may significantly increase the accessibility of electrocatalytically active sites.57
It is therefore necessary to analyze the elemental composition of the sample to further confirm the existence of this effect. The elemental analysis was conducted through an energy-dispersive X-ray spectroscopy (EDS) analysis using an electron microscope (Fig. S2–S5†). From these figures, it is evident that the distribution of the carbon element and the carbon skeleton is highly consistent, confirming the presence of a continuous conductive pathway in the material. The MnNiCu element in the prepared (MnNiCu)F2-PCNFs, the MnNiCuCo element in (MnNiCuCo)F2-PCNFs, the MnNiCuZn element in (MnNiCuZn)F2-PCNFs and the MnNiCuCoZn element in (MnNiCuCoZn)F2-PCNFs all overlap with each other. The fluorine element in each sample is distributed on the skeleton and aggregated at the particles. These pieces of evidence together strongly prove the successful synthesis of multi-metallic fluorides. When comparing the content of each element (Table S2†), carbon still accounts for the absolute majority (>90%), which is rather beneficial to the smooth transmission of electrons. The fluorine element is more than twice that of each metal element, which greatly proves that in addition to metal fluorides, some fluorine is combined with carbon to form fluorine-doped carbon materials. In order to facilitate the comparison of the content of metal elements, the content of each metal element is obtained and depicted in a pie chart (Fig. 3a). It can be seen that the MnNiCu element in (MnNiCu)F2-PCNFs and the MnNiCuCo element in (MnNiCuCo)F2-PCNFs both show comparable proportions. The MnNiCuZn element in (MnNiCuZn)F2-PCNFs and the MnNiCuCoZn element in (MnNiCuCoZn)F2-PCNFs both show a slightly lower proportion of Zn than MnNiCuCo, and MnNiCuCo are comparable proportions. These test results also further confirm that zinc will be partially lost during the preparation process. In addition, based on previous research reports, the configurational entropy of the obtained (MnNiCu)F2-PCNFs, (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCuCoZn)F2-PCNFs can be calculated using Formula S3† based on the data from Fig. 3a, which are 1.09R, 1.39R, 1.36R, and 1.60R, respectively.58 Among them, the configurational entropy of (MnNiCuCoZn)F2-PCNFs is larger than 1.5R, which can be identified as high-entropy fluorides among these samples.23,59
Fig. 3 (a) The content of each metal element in the sample (atomic%). (b) The X-ray diffraction (XRD) pattern. (c) The nitrogen adsorption–desorption curves and (d) pore size distribution diagrams. |
The XRD patterns of the sample is shown in Fig. 3b, and the (MnNiCuCoZn)F2 model can be constructed according to the metal element ratio of the obtained (MnNiCuCoZn)F2-PCNFs. The simulated (MnNiCuCoZn)F2 has an XRD pattern similar to that of the actual (MnNiCuCoZn)F2-PCNFs, which significantly illustrates successful synthesis of (MnNiCuCoZn)F2-PCNFs. The prepared (MnNiCuCoZn)F2-PCNFs exhibit similar independent peaks when compared to the standard card of monometallic fluorides. Compared to the superimposed XRD spectra of individually prepared single-metal fluoride composite PCNFs, the XRD spectra measured from (MnNiCuCoZn)F2-PCNFs are significantly more consistent with the simulated XRD spectra (Fig. S6†). These results show that it is a new type of fluoride crystal different from single metal fluoride, rather than a simple physical mixture of individual single metal fluorides. The obtained MEF-PCNFs with three or four metal element types have different lattice distortion effects from the obtained (MnNiCuCoZn)F2-PCNFs due to some differences in the atomic radii of the metal elements. Therefore, they will exhibit inconsistent crystal constants and slightly different XRD patterns.25
The pore structure of the material was also tested and characterized through the nitrogen adsorption and desorption curves (Fig. 3c). The corresponding pore size distribution is also given in Fig. 3d. The specific surface area of (MnNiCu)F2-PCNFs, (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCuCoZn)F2-PCNFs is 166.4 m2 g−1, 153.0 m2 g−1, 127.5 m2 g−1 and 101.0 m2 g−1, respectively. That is, when the metal component is more, it is more likely to block a wider range of micropores.60 When compared with micropores and macropores, mesopores have more advantages in mass transfer, gas transport and liquid electrolyte penetration.61,62 The mesopore volumes for (MnNiCu)F2-PCNFs, (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCuCoZn)F2-PCNFs are 0.284 cc g−1, 0.252 cc g−1, 0.285 cc g−1, and 0.275 cc g−1, respectively. The mesoporous fraction of (MnNiCuCoZn)F2-PCNFs, with the highest being 0.285 cc g−1, differed by less than 5%. Referring to related work already reported, it can be inferred that the mesoporous structure of (MnNiCuCoZn)F2-PCNFs is approximately equivalent to that of the other samples to a certain extent.63–66
The binding energies (B.E.) can be tested through X-ray photoelectron spectroscopy (XPS) for composition characterization and the electronic state (Fig. 4 and S7†). The deconvolution results of Mn-2p show that the Mn-2p3/2 of each sample appears at around 642.7 eV, among which the Mn-2p3/2 of (MnNiCuCo)F2-PCNFs shifts positively by 0.1 eV when compared to that of other samples. The deconvolution results of Ni-2p show that the B.E. of Ni-2p2/3 in the (MnNiCu)F2-PCNF increases from 857.2 eV to 857.5 eV and 857.4 eV in the case of Co and Zn doping, respectively. When Co and Zn are doped at the same time, the B.E. of Ni-2p3/2 further shifts positively to 857.7 eV, which shows that the doping of Co and Zn can further reduce the electron density of nickel in multi-component fluorides. Some studies suggest that this reduction in electron density is beneficial to the progress of nucleophilic reactions (such as the OER under alkaline conditions).67,68 The B.E. of Cu-2p3/2 moves negatively from 934.1 eV of the prepared (MnNiCu)F2-PCNFs to 933.5 eV of the obtained (MnNiCuCo)F2-PCNFs, 933.8 eV of the prepared (MnNiCuZn)F2-PCNFs and 933.8 eV of the obtained (MnNiCuCoZn)F2-PCNFs, respectively.69 These test results also reflect that the electron density of copper atoms can be increased due to the doping of Co and Zn to greatly promote electrophilic reactions (such as the ORR under alkaline conditions).67 A relatively obvious Co-2p3/2 peak can be identified in both the prepared (MnNiCuCo)F2-PCNFs and (MnNiCuCoZn)F2-PCNFs near 782.5 eV.70 For the (MnNiCuZn)F2-PCNFs and (MnNiCuCoZn)F2-PCNFs, the Zn-2p3/2 peak is identified near 1022.4 eV, which strongly reflects that successful doping of Zn can be realized.71 The F-1s energy spectra of all samples can be decomposed into C–F bonds at 687.0 eV and ionic metal-fluorine bonds (M−F) at 684.7 eV.72
Fig. 4 High-resolution X-ray photoelectron spectra. (a) Mn-2p, (b) Ni-2p, (c) Cu-2p, (d) Co-2p, (e) Zn-2p, and (f) F-1s. |
The ORR activities of the prepared catalysts are measured using a typical three-electrode system in 0.1 M KOH, where all potentials are calibrated to the potential relative to RHE. The polarization current curves and the corresponding Tafel slopes are shown in Fig. 5a and b. As for (MnNiCuCoZn)F2-PCNFs, the onset potential (E0) is 0.899 V, the half-wave potential (E1/2) is 0.852 V, and the limit current density (JL) is 5.52 mA cm−2. The ORR activities of (MnNiCuCoZn)F2-PCNFs are slightly lower than that of the commercial Pt/C catalyst (E0 = 0.926 V, E1/2 = 0.856 V, and JL = 5.50 mA cm−2), but these performances are superior to those of the (MnNiCuZn)F2-PCNFs (E0 = 0.883 V, E1/2 = 0.740 V, and JL = 4.84 mA cm−2), the (MnNiCuCo)F2-PCNFs (E0 = 0.875 V, E1/2 = 0.782 V, and JL = 4.35 mA cm−2), and the (MnNiCu)F2-PCNFs (E0 = 0.831 V, E1/2 = 0.758 V, and JL = 3.49 mA cm−2). When compared to the (MnNiCu)F2-PCNFs, the obtained (MnNiCuZn)F2-PCNFs exhibit a higher E0 and a significant improvement in JL. Therefore, it is speculated that the addition of zinc components significantly enhances the variety and number of active sites in the prepared (MnNiCuZn)F2-PCNFs. Moreover, the (MnNiCuCo)F2-PCNFs show higher E0, E1/2, and JL when compared to the (MnNiCu)F2-PCNFs, indicating that the incorporation of cobalt components significantly enhances the intrinsic activity and quantity of ORR active sites in the (MnNiCuCo)F2-PCNFs. Unlike the dispersed pore size distribution of (MnNiCuZn)F2-PCNFs, the (MnNiCuCo)F2-PCNFs constructed a more concentrated mesoporous structure with a pore size of about 5 nm, which may be related to the enhancement of ORR intrinsic activity. The obtained (MnNiCuCoZn)F2-PCNFs exhibit a combination of the features of (MnNiCuCo)F2-PCNFs and (MnNiCuZn)F2-PCNFs, forming a concentrated mesoporous structure with a 5 nm pore size and transformed fluoride crystals. The formed unique structure endows the prepared (MnNiCuCoZn)F2-PCNFs with enhanced ORR intrinsic activity and more ORR active sites. The Tafel slope of (MnNiCuCoZn)F2-PCNFs is 83.4 mV dec−1, which is lower than that of the (MnNiCuCo)F2-PCNFs (96.5 mV dec−1), the (MnNiCuZn)F2-PCNFs (112.6 mV dec−1), the (MnNiCu)F2-PCNFs (101.8 mV dec−1), and even the commercial Pt/C (96.5 mV dec−1), suggesting that the (MnNiCuCoZn)F2-PCNFs exhibit rapid ORR kinetics.73 Furthermore, as shown in Fig. S8,† the n value of (MnNiCuCoZn)F2-PCNFs is approximately 4, which is higher than that of the obtained (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCu)F2-PCNFs, indicating that a high four-electron selectivity towards the ORR for (MnNiCuCoZn)F2-PCNFs can be obtained.74
For the OER (Fig. 5c and d), the (MnNiCuCoZn)F2-PCNFs exhibit an overpotential (η10 = Ej=10 − 1.23 V) of 310 mV, which is lower than that of RuO2 (318 mV), the (MnNiCuCo)F2-PCNFs (368 mV), the (MnNiCuZn)F2-PCNFs (391 mV), and the (MnNiCu)F2-PCNFs (385 mV). When compared to the (MnNiCu)F2-PCNFs, the (MnNiCuZn)F2-PCNFs show an increased η10 but also a higher current density at 1.65 V, suggesting that the introduction of Zn can increase the number of OER active sites in the (MnNiCuZn)F2-PCNFs, but with a slightly weaker intrinsic activity. The results can be mainly attributed to some differences in pore size distribution and particle integrity between the (MnNiCuZn)F2-PCNFs and the (MnNiCu)F2-PCNFs. The introduction of Co in the (MnNiCuCo)F2-PCNFs results in a lower η10 and a higher current density at 1.65 V vs. RHE compared to the (MnNiCu)F2-PCNFs, reflecting the enhanced intrinsic OER catalytic activity due to Co incorporation. The synergistic effect of Co and Zn components in the (MnNiCuCoZn)F2-PCNFs leads to a significantly lower η10 and enhanced current density at 1.65 V vs. RHE compared to those of the (MnNiCuCo)F2-PCNFs, the (MnNiCuZn)F2-PCNFs, and the (MnNiCu)F2-PCNFs. Comparison of the Tafel slopes reveals the following order: (MnNiCuCoZn)F2-PCNFs (88.2 mV dec−1) < (MnNiCuCo)F2-PCNFs (89.1 mV dec−1) < (MnNiCu)F2-PCNFs (93.8 mV dec−1) < (MnNiCuZn)F2-PCNFs (97.0 mV dec−1), which is in complete agreement with the above analysis and further confirms the synergistic effect of Co and Zn components. The Tafel slope of (MnNiCuCoZn)F2-PCNFs, being lower than that of RuO2 (130.3 mV dec−1), also demonstrates its superior OER kinetics.75,76 After 2000 cycles of accelerated durability testing (ADT), the η10 of (MnNiCuCoZn)F2-PCNFs increases by 18 mV, whereas that of RuO2 increases by 20 mV (Fig. S9†), indicating that a stable and excellent OER performance of (MnNiCuCoZn)F2-PCNFs can be realized.
The electrochemical surface area (ECSA) is defined as the actual effective area on the electrode material that can participate in electrochemical reactions.77 The parameter is crucial for assessing the electrocatalytic efficiency of electrode materials, as the rate of electrochemical reactions is typically directly related to the material's effective surface area.78,79 The capacitance value is obtained by calculating at different scan rates within the non-faradaic current range. The CV curves at different scan rates within the non-faradaic current range for these prepared (MnNiCu)F2-PCNFs, (MnNiCuCo)F2-PCNFs, (MnNiCuZn)F2-PCNFs, and (MnNiCuCoZn)F2-PCNFs are shown in Fig. S10.† Fitting the central intercept of their CV curves yields their double-layer capacitance (Cdl) (Fig. 5e). The Cdl of (MnNiCuCoZn)F2-PCNFs is 17.6 mF cm−2, which is essentially equivalent to the 18.3 mF cm−2 of (MnNiCuZn)F2-PCNFs, and higher than the 12.0 mF cm−2 of (MnNiCuCo)F2-PCNFs and the 8.7 mF cm−2 of (MnNiCu)F2-PCNFs, indicating that zinc contributes more to the Cdl than cobalt. The reason is speculated to be related to zinc inducing a polycrystalline transition in the fluoride, leading to more accessible electrochemical reaction sites.39 Based on the measurement results of Cdl, the ECSA was calculated and used to normalize the OER catalytic performance.80,81 The normalized polarization curves from the ECSA also revealed the superiority of the (MnNiCuCoZn)F2-PCNFs among these samples (Fig. S11†).80 Electrochemical Impedance Spectroscopy (EIS) is employed to reveal the charge transfer capabilities of the prepared catalysts and to discuss their impact on the electrocatalytic activity. The measured Nyquist plots, as shown in Fig. S12,† generally indicate a positive correlation between the semicircle diameter and the charge transfer impedance.82 Consequently, the order of magnitude for charge transfer impedance is as follows: (MnNiCuCoZn)F2-PCNFs < (MnNiCuCo)F2-PCNFs < (MnNiCu)F2-PCNFs < (MnNiCuZn)F2-PCNFs. This order inversely correlates with their OER activity trends, suggesting that smaller charge transfer impedance is conducive to faster OER kinetics.83
Structural stability is crucial for the catalytic performance of catalysts. The long-term stability of (MnNiCuCoZn)F2-PCNFs for the OER was tested as shown in Fig. S13.† The prepared (MnNiCuCoZn)F2-PCNFs exhibited a 94% current density, which was significantly superior to the 76% of RuO2. The XRD test result of (MnNiCuCoZn)F2-PCNFs after a 20000-second OER process also confirmed that the stable existence of high-entropy fluorides can be obtained (Fig. S14†). Moreover, the microstructure of (MnNiCuCoZn)F2-PCNFs after the OER process was carefully observed using the HR-TEM testing equipment (Fig. S15†). The prepared (MnNiCuCoZn)F2-PCNFs still displayed their original nanofiber conductive pathways even after the OER (Fig. S15a†). Additionally, the polycrystalline structure of the high-entropy fluorides was demonstrated by the rotation of electron diffraction spots in the SAED pattern (Fig. S15b2†).54–56 Furthermore, a linear scanning of EDS on the (MnNiCuCoZn)F2-PCNFs after the OER also revealed that a distinct high-intensity signal of the oxygen element at the crystal interfaces of the polycrystalline (MnNiCuCoZn)F2 particles can be realized (Fig. S15d†). All of these proved that the crystal interfaces of the polycrystalline particles were more likely to participate in the OER, thereby generating oxygen-containing intermediates.84
The practical application of the prepared catalysts is evaluated by assembling them into ZABs (Fig. 5f). Initially, their discharge polarization curves are obtained, and the power density curves are obtained (Fig. 5g). The (MnNiCuCoZn)F2-PCNF-based-ZAB exhibits a peak power density of 206 mW cm−2, which is higher than that of the (MnNiCuZn)F2-PCNF-based-ZAB (178 mW cm−2), the (MnNiCuCo)F2-PCNF-based-ZAB (151 mW cm−2), and the (MnNiCu)F2-PCNF-based-ZAB (127 mW cm−2), and even surpasses that of the Pt/C + RuO2-based-ZAB (172 mW cm−2). These results demonstrate the effective power release capability of the (MnNiCuCoZn)F2-PCNFs as a cathode catalyst for ZABs. As depicted in Fig. 5h, the (MnNiCuCoZn)F2-PCNF-based-ZAB exhibits a specific capacity of 760 mA h g−1, exceeding that of the (MnNiCuZn)F2-PCNF-based-ZAB (611 mA h g−1), the (MnNiCuCo)F2-PCNF-based-ZAB (647 mA h g−1), and the (MnNiCu)F2-PCNF-based-ZAB (555 mA h g−1), and even outperforming the Pt/C + RuO2-based-ZAB (682 mA h g−1). All of these results reflect the highest specific capacity output capability of the (MnNiCuCoZn)F2-PCNFs as a cathode catalyst for ZABs among the prepared samples. Moreover, the (MnNiCuCoZn)F2-PCNF-based-ZAB is able to operate for over 400 h (Fig. 5i), significantly surpassing the Pt/C + RuO2-based-ZAB. In comparison to some related studies reported in Table S3,† the (MnNiCuCoZn)F2-PCNFs prepared in this study exhibited a superior potential gap (ΔE = Ej=10 − E1/2 = 0.688 V) and a higher peak power density of 206 mW cm−2. This demonstrates the broad application prospects of the (MnNiCuCoZn)F2-PCNFs as bifunctional oxygen electrocatalysts.
For understanding the impact of electronegativity differences among various metals in HEAs on driving the adsorption and conversion of intermediates in alkaline ORR and OER, we proposed the potential adsorption state models and schematic diagrams of reaction processes based on classical electrochemical oxygen catalysis theory.53,85 As shown in Fig. 6a, under alkaline conditions, the OER process involves the interaction of H2O with the catalyst, successively generating *OH, *O, and *OOH transition states, eventually converting to O2.86 The ORR process is the reverse reaction of the OER process, where the interaction of O2 with the catalyst successively generates *OOH, *O, and *OH transition states, eventually converting to H2O. Based on the results of the preliminary component analysis, a structural model with a constant metal atom ratio (MnNiCuCoZn)F2 was constructed, as shown in Fig. 6b.
Based on the results of preliminary compositional analysis, we constructed a model with a constant metal atomic ratio, (MnNiCuCoZn)F2, exhibiting a tetragonal symmetry structure. The (MnNiCuCoZn)F2 model with tetragonal symmetry is shown in Fig. 6b. It is generally believed that oxygenated transition states will only adsorb on metal atomic sites, so we conducted an analysis of the partial density of states (PDOS) for the metal elements (Fig. 6c and d). Compared to the isolated density of electronic states near EF in (MnNiCuCo)F2, (MnNiCuCoZn)F2 exhibits a continuous distribution of electronic states near EF, which further illustrates that the low charge transfer resistance of (MnNiCuCoZn)F2 can be obtained.87,88
The ORR process involves the dissociation of the O–O bond in O2 and adsorption on the metal site surface, followed by multiple protonation steps to form oxygenated intermediates (i.e., *OOH, *O, and *OH) and H2O.89 The adsorption energies for each possible step on each metal site of (MnNiCuCoZn)F2 are shown in Fig. 7a, with each energy value corrected through U = −1.23 V to eliminate the effect of the standard potential.53 The calculated results indicate that the energy barrier of the rate-determining step (RDS) on the Co site exhibits a ΔG value of 0.60 eV, which is lower than those on Zn (ΔG = 3.33 eV), Cu (ΔG = 0.80 eV), Ni (ΔG = 3.92 eV), and Mn (ΔG = 1.80 eV) sites. Therefore, Co sites in (MnNiCuCoZn)F2 can offer better ORR catalytic activity when compared to other metal sites. The RDS energy barrier on Zn sites is significantly higher than those on Cu and Co, indicating that the ORR activity contributed by Zn sites is very limited. Additionally, a model with a constant metal atomic ratio for (MnNiCuCo)F2 is also constructed and the derived oxygenated intermediates for each metal site are simulated to obtain the energy distribution (Fig. 7b). The comparison between (MnNiCuCo)F2 and (MnNiCuCoZn)F2 helps elucidate the role of Zn components in mid-entropy fluorides. Herein, Co sites exhibit the lowest energy barrier for the RDS in the ORR (ΔG = 1.03 eV) among these samples, which is lower than those for Cu (ΔG = 2.87 eV), Ni (ΔG = 1.65 eV), and Mn (ΔG = 2.34 eV). The addition of Zn components leads to a reduction in the energy of derived oxygenated intermediates on Co sites of (MnNiCuCoZn)F2, with the RDS involving the protonation move from *OOH to *OH. The results further lead to a significantly lower ΔG value for Co sites in (MnNiCuCoZn)F2 when compared to (MnNiCuCo)F2, strongly proving that the higher ORR activity of (MnNiCuCoZn)F2 also stems from Zn's improvement of the electronic structure. Hence, Co components dominate the ORR catalytic process in the (MnNiCuCoZn)F2-PCNFs. Besides affecting the pore structure characteristics of PCNFs and causing transformation of the (MnNiCuCoZn)F2 nanoparticles to expose more active sites, zinc's role in electronic regulation on other metal sites can further enhance ORR catalytic activity.
Fig. 7 The adsorption energy distribution diagram of each metal site on (MnNiCuCoZn)F2 and (MnNiCuCo)F2. The (a and b) ORR process and (c and d) OER process. |
The OER process involves the adsorption of H2O on the surface of metal sites, followed by multiple deprotonation steps and O–O coupling to form oxygenated intermediates (i.e., *OH, *O, and *OOH) and O2.89 The OER processes of (MnNiCuCoZn)F2 and (MnNiCuCo)F2 are shown in Fig. 7c and d. The deprotonation of *OH to form the *O species, as well as the combination of *O with H2O and subsequent deprotonation to form *OOH species, may be challenging and act as the possible RDS (Rate-Determining Steps) for metal sites in both (MnNiCuCo)F2 and (MnNiCuCoZn)F2. The energy barrier of the RDS on the Co site of (MnNiCuCoZn)F2 exhibits a ΔG value of 0.73 eV, which is lower than those on Zn (ΔG = 2.31 eV), Cu (ΔG = 1.06 eV), Ni (ΔG = 1.84 eV), and Mn (ΔG = 3.19 eV) sites. Therefore, the Co site can contribute to higher OER catalytic activity when compared to other metal sites in (MnNiCuCoZn)F2. The energy barriers of the RDS for various metal atoms in (MnNiCuCo)F2 are Co (ΔG = 1.35 eV), Cu (ΔG = 1.84 eV), Ni (ΔG = 2.36 eV), and Mn (ΔG = 4.92 eV), respectively. The Co component in both (MnNiCuCo)F2 and (MnNiCuCoZn)F2 exhibits a vital role in the OER process. These results indicate that Zn significantly reduces the activation energy required for the deprotonation of *OH on Co atoms (1.35 eV → 0.73 eV), thereby significantly enhancing the OER kinetics of (MnNiCuCoZn)F2.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ta02866j |