Mandeep
Singh
a,
Francesco
Scotognella
*b and
Giuseppe Maria
Paternò
*a
aPhysics Department, Politecnico di Milano, Piazza L. da Vinci 32, 20133 Milano, Italy. E-mail: francesco.scotognella@polito.it
bDepartment of Applied Science and Technology, Politecnico di Torino, Corso Duca degli Abruzzi 24, Torino 10129, Italy. E-mail: giuseppemaria.paterno@polimi.it
First published on 1st August 2024
The tuneability of the localized surface plasmon resonance (LSPR) of degenerately doped metal oxide (MOX) nanocrystals (NCs) over a wide range of the infrared (IR) region by controlling NC size and doping content offers a unique opportunity to develop a future generation of optoelectronic and photonic devices like IR photodetectors and sensors. The central aim of this review article is to highlight the distinctive and remarkable plasmonic properties of degenerately or heavily doped MOX nanocrystals by reviewing the comprehensive literature reported so far. In particular, the literature of each MOX NC, i.e. ZnO, CdO, In2O3, and WO3 doped with different dopants, is discussed separately. In addition to discussion of the most commonly used colloidal synthesis approaches, the ultrafast dynamics of charge carriers in NCs and the extraction of LSPR-assisted hot-carriers are also discussed in detail. Finally, future prospective applications of MOX NCs in IR photodetectors and photovoltaic (PV) self-powered chemical sensors are also presented.
The discovery of LSPR in degenerately doped MOX nanocrystals (NCs) such as aluminium-doped ZnO (AZO), tin-doped indium oxide (ITO), or WO3, opens up a new possibility for developing a future generation of optoelectronic and photonic devices.1,9,10 LSPR in doped semiconductors holds an advantage over metal nanoparticles because their LSPR can be tuned from the THz to the NIR region by controlling the doping level and NC size, as shown in Fig. 1.11 This is a two-dimensional Drude–Lorentz plot of NC size vs. LSPR frequency. As can be seen from Fig. 1, for degenerately doped semiconductors, by controlling the doping concentration between 1019 and 1021 cm−3, the LSPR can be tuned from the far infrared (FIR) to the near-infrared (NIR) region. The wide range of tuneability over the IR region makes degenerately doped semiconductors interesting for optoelectronics, photonics, and biomedical applications.12–14 Furthermore, most MOXs, such as ZnO, CdO, In2O3, and WO3, are intrinsically n-type doped semiconductors due to the presence of oxygen vacancies; thus they exhibit LSPR features even when no external doping has been done.2 The prime example of this is WO3−x NCs.15
Fig. 1 Localized surface plasmon resonance (LSPR) frequency dependence on free carrier density and doping constraints. Reproduced from ref. 11 with permission from Springer Nature, copyright 2011. |
This review article is focused on highlighting the plasmonic properties of MOX NCs by reviewing the significant literature reported so far and their future prospective application in IR photodetectors and PV self-powered sensors. While reviewing the literature, we have tried to include all those reports in which interesting synthetic conditions or strategies were used to tune and improve the plasmonic properties of MOX NCs. We would like to point out that for a detailed and deeper understanding of different types of degenerately doped semiconducting materials and their fundamental plasmonic properties, readers can refer to the comprehensive review article by Milliron and collaborators.2 Here, we first discuss the properties which make MOX NCs unique materials for harvesting light from a wide solar spectrum (UV-vis-IR) and provide an overview of the ultrafast charge-carrier dynamics along with the extraction of LSPR-assisted hot-carriers. Then, we present the most commonly used colloidal methods to synthesise NCs with relevant examples and review the comprehensive literature on degenerately doped indium oxide (In2O3), zinc oxide (ZnO), cadmium oxide (CdO) and tungsten oxide (WOx) NCs. Finally, prospective applications of NCs in IR photodetectors and PV self-powered sensors are presented.
Recently, it has been observed that photogeneration of charge carriers occurs in MOXs under visible-light excitation.22 This phenomenon is significantly explored in tuning the selectivity and response of gas sensors.22,23 Q. Geng et al.24 have illuminated ZnO with visible light ranging from 420 nm to 520 nm from an LED source and observed the sensing response owing to the photogenerated charge carriers. They have associated photogeneration in visible light with the phenomenon of two-photon or multi-photon absorption.25,26 Detailed discussion of these phenomena is outside the scope of this review.
Finally, the LSPR in heavily doped MOX NCs in IR, which is the main topic of this review article, extends the light-harvesting capability of MOXs to the IR region. Later in the review article we will discuss the prospective application of MOX NCs for a future generation of IR-photodetectors and photovoltaic (PV) self-powered sensors due to their ability to harvest energy from a wider range of the solar spectrum (UV-vis-IR). However, to use degenerately doped MOX NCs for these two applications required a deeper understanding of their plasmonic dynamics under the illumination of IR-radiation and suitable device configuration for plasmon-assisted hot-carrier extraction. This leads us to our next section in which both these aspects are discussed.
In this regard, Kriegel et al.36 investigated the ultrafast photodoping and plasmon dynamics in fluorine–indium co-doped CdO (FICO) NCs via pumping at 400 nm (band-gap excitation) and 1350 nm (LSPR excitation). The NCs were prepared by the heat-up method and the measurements were performed on a suspension of NCs in different solvents. Fig. 2 represents the transient-absorption (TA) response of FICO NCs to the intraband excitation of LSPR at 1350 nm. In particular, Fig. 2a shows the derivative-shaped TA spectra at a time-delay of 0.1 ps (left) along with the two-dimensional map of ΔT/T(%) (right). Two types of contribution were observed: the maximum of the TA spectra (indicated by a broken blue line), represents photobleaching (PB) and photoinduced absorption (PA) is indicated by a broken red line. In Fig. 2b the decay of both PB and PA at 1580 nm and 1650 nm is shown. Two well-separated time-dependent dynamics were observed when NCs were excited with LSPR resonance: short-dynamics in the picosecond time range and longer-dynamics from 10 to 100 picoseconds. The initial fast decay (1 ps) is associated with the emission of phonons (carrier-phonons) and the slower decay corresponds to phonon–phonon scattering and the dissipation of heat into the solvent. It was also indicated that the initial fast decay was in fact even faster than that with noble metals due to the lower heat capacity and carrier concentration of semiconductor NCs. On the other hand, the TA dynamics of NCs after band-gap excitation (400 nm) is shown in Fig. 3. As shown in Fig. 3a, reverse dynamics as compared to LSPR excitation is observed. The PB maximum was observed at 1625 nm, while the negative signal (PA) showed a peak value at 1550 nm. Furthermore, the time axis in two-dimensional LSPR excitation (Fig. 2a) was up to 2 ps, while it was 10 ps in the case of 400 nm excitation, indicating that faster dynamics and signal modulation occurred when the NCS were excited at 1350 nm. A monoexponential decay in the signal was observed after the short rise time. The authors argued that pumping at 400 nm results in the excitation of electrons to the conduction band, which increases the carrier density by capacitive charging. They proposed that the observed monoexponential decay is due to the temporarily increased carrier density after the ultrafast photodoping, which decays via electron−hole recombination.
Fig. 2 Transient optical response of FICO NCs following intraband excitation. (a) Representative TA spectrum at the maximum rise time of around 100 fs after photoexcitation, exhibiting a derivative-shaped curve (left) together with the two-dimensional ΔT/T map (right), showing the signal as a function of pump–probe delay and probe wavelength for FICO NCs excited at 1350 nm with an excitation density of 0.13 mJ cm−2. The steady-state LSPR absorption spectrum is also given in grey for comparison. (b) Transient decay dynamics at 1580 nm together with a biexponential fit (blue and black curves, respectively; upper panel, time constants of 0.23 and 38 ps) and 1650 nm (red curve, lower panel), illustrated by the horizontal cuts (dashed lines) depicted in panel (a). The time constant of the initial fast decay at 1650 nm is around 0.15 ps (not shown here). (c) ΔT/T time traces extracted at the selected probe wavelengths to the red (around 1655 nm) and the blue (1500 nm) of the maximum PB signal after subtracting the biexponential decay, along with their fits by a damped sinusoidal function (black curves). The extracted oscillating period is T = 4.4 ps, and the damping time constant is τ = 7 ps. Reproduced from ref. 36 with permission from ACS, copyright 2016. |
Fig. 3 Transient optical response of FICO NCs following intraband excitation. (a) TA spectrum at the maximum signal (0.6 ps) showing the typical derivative-shaped curve together with the two-dimensional ΔT/T map showing the signal as a function of pump–probe delay and probe wavelength for FICO NCs excited at 400 nm for the excitation density 2.35 mJ cm−2. The steady-state LSPR absorption spectrum is also given in gray for comparison. (b) Transient decay dynamics at 1625 nm (blue curve upper panel) and 1550 nm (red curve lower panel) together with the monoexponential fits (black curve, time constant of 1.7 ps), illustrated by the horizontal cuts (dashed lines) depicted in panel a. Reproduced from ref. 36 with permission from ACS, copyright 2016. |
In another study, In and Al-doped ZnO NCs were explored for ultrafast and broadband mid-infrared all-optical switching.37 The In-doped ZnO NCs were synthesized using the heat-up method while the Al-doped ZnO NCs were synthesized using hot-injection. Briefly, by pumping NCs with LSPR resonance, picosecond all-optical Q-switching was realized with doped ZnO NCs in the MIR region from 3 to 5 μm.
Furthermore, the practical use these plasmonic properties of doped-MOX NCs relies mainly on the extraction of LSPR-assisted hot-electrons. However, hot-electrons exhibit very short lifetimes (tens of femtoseconds in metal38 and hundreds of femtoseconds in doped oxide NCs36), making them difficult to extract. The extraction of these hot-carriers requires a suitable device structure or a junction with a suitable extraction layer. One such effort was made by M. Guizzardi et al.39 in which the extraction of hot-carriers was done by fabricating a heterostructure between ITO NCs and a monolayer of molybdenum disulfide (MoS2). The ITO NCs were synthesized by the continuous growth method and were transferred to the MoS2 monolayer with spin-coating. Fig. 4 shows a depiction of the ITO/MoS2 heterojunction and the band alignment between ITO and MoS2. The heterostructure was pumped in resonance with the LSPR of ITO NCs at 1750 nm which was well below the band gap of MoS2. By pumping the LSPR, a charge transfer from ITO to MOS2 was observed that makes these types of heterostructure interesting for light-harvesting devices like infrared-solar cells.
Fig. 4 (a) ITO/MoS2 heterojunction sketch. (b) Band alignment between ITO and MoS2; on the right-hand side, we have the sketch of the hot Fermi–Dirac distribution. Reproduced from ref. 39 with permission from ACS, copyright 2022. |
After discussing plasmonic dynamics in NCs, we reach a point where it is necessary discus the synthetic approaches that are used to synthesize these plasmonic materials.
For the synthesis of plasmonic MOX NCs, three main colloidal synthetic route routes have been very commonly used, namely:
(a) Hot-injection method.
(b) Heat-up method.
(c) Continuous growth method (slow injection).
The typical experimental setup for NC synthesis is composed of a three-neck round-bottom flask, a heating mantle with a temperature controller (inserted into the NC solution) and syringe for injection of the reactant. As the synthesis is done in under inert environmental conditions (e.g. in nitrogen), the middle neck is connected to a Schlenk line. A schematic of the setup is shown in Fig. 5a.2
Fig. 5 General synthetic apparatus and growth model embodying the colloidal synthetic technique. (a) Schematic showing glassware and peripheral instrumental setup for a typical synthesis of surfactant-stabilized NCs, involving hot-injection. (b) LaMer–Dinegar model of colloidal NC formation. The three stages of monomer generation, nucleation, and growth are demarcated in the regions below the growth curve along with cartoons depicting the progression of the synthesis. Reproduced from ref. 2 with permission from ACS, copyright 2018. |
Before we go into the detail of these methods, it is important to understand the nucleation and growth of NCs that were explained by LaMer and Dinegar in 1950.40 In particular, they investigated the development of sulfur hydrosol for the slow decomposition of dilute sodium thiosulfate in dilute hydrochloric acid. Basically, it consists of three stages: monomer generation, nucleation and finally the growth of NCs (Fig. 5b).2 In the first stage, the precursor is dissolved in the solvent and the reaction between them leads to the formation of a monomer.
The rate of monomer generation depends on the reaction kinetics and temperature. As the reaction proceeds, the concentration of monomer reaches its saturation level (Cs) and at this point nucleation does not start immediately as there is still a significant barrier to nucleation. However, when the monomer concentration reaches a certain minimum level (Cnumin), nucleation starts spontaneously. During the accelerated growth of nuclei, the monomer is abruptly consumed. In fact, the monomer is formed by aggregation and self-nucleation processes. As the temporal formation of nuclei goes on, the monomer concentration reaches supersaturation and drops instantaneously. Indeed, the nucleation process stops when it reaches the Cnumin level, which is the onset of the third and final stage: i.e. the growth of NCs via aggregation of monomers on pre-existing nuclei.
Now, let us come back to the three NC synthesis methods. All three methods are similar to each other as far as the overall process is concerned, but the major difference lies in the occurrence of nucleation and growth.2
With this method, Sirshendu Ghosh et al.42 fabricated indium (In)-doped ZnO NCs in a nanopyramid shape, as shown in Fig. 6. The whole synthesis process is as follows: 2 mM of zinc acetylacetonate and indium acetate with different molar ratios were mixed with 2 mmol oleic acid and 5 mL of 1-octadecene (ODE) in a three-neck round-bottom flask. The mixture was first vacuumed at room-temperature and finally heated to 90 °C under the flow of Ar gas. Afterward, 15 mM of oleyl amine was dissolved in 1 mL of ODE and injected into the flask. The mixture was heated for 60 minutes at 240 °C, leading to the formation of In-doped ZnO NCs with broad LSPR in the IR region.
Fig. 6 (a) FESEM image of pure ZnO. (b) Low-resolution TEM image of the pure ZnO nanopyramid. The top-left and bottom-right insets of the figure depict the tilted (X = 41.1°, Y = 0°) and side views of a single ZnO hexagonal nanopyramid. (c) SAED pattern of the nanopyramid. (d) A single hexagonal pyramid viewed from the (0001) zone axis. (e) SAED pattern of a single nanocrystal. (f) Schematic presentation of a nanopyramid. (g) HRTEM image of a nanocrystal at the cross-section of two edges of the base. The inset shows the corresponding FFT pattern of the area. (h) Side view of a nanopyramid. (i) HRTEM image of the tip of the pyramid. (j) HRTEM image of the base of the pyramid. Reproduced from ref. 42 with permission from RSC, copyright 2014. |
This method is extremely useful for applications in which precise control over the physical properties of NCs is required, i.e. the exploitation of LSPR. However, hot-injection is not useful for large-scale production, due to its dependency on the homogeneous mixing of reactants in a short period of time at high temperature; cooling can be inhomogeneous if the reaction is performed in a large reactor and a large volume of reactant cannot be injected abruptly, which can lead to the fabrication of inhomogeneous NCs with a broad range of sizes.2
Fig. 7 (a) Schematic illustration of the hot-injection method and heat-up method for uniform-sized nanoparticles. (b) Transmission electron microscopy (TEM) image of 11 nm γ-Fe2O3 nanoparticles. (c) The overall scheme for the synthesis of monodispersed nanoparticles through metal–oleate complexation. (d) TEM image of 12 nm Fe3O4 nanoparticles. Inset is a photograph of 40 g of the monodispersed Fe3O4 nanoparticles, and a US one-cent coin for comparison. (e) Photograph of Taeghwan Hyeon and Jongnam Park in 2004. (f)–(h) TEM images of (f) 6 nm, (g) 12 nm, (h) 10 nm monodispersed Fe3O4 nanoparticles. Reproduced from ref. 44 with permission from Wiley, copyright 2023. |
Fig. 8 TEM images taken of doped In2O3 nanocrystals at varying molar dopant ratios. Scale bars are 20 nm. The nominal dopant percent in the precursor increases from left to right, 5% dopant on the left, 10% center, and 20% right: (a) Mn:In2O3, (b) Fe:In2O3, (c) Co:In2O3, (d) Cu:In2O3, and (e) Zn:In2O3. Reproduced from ref. 45 with permission from ACS, copyright 2017. |
Fig. 9 Solution-phase UV-vis-IR absorbance spectra of four shapes (spheres, triangles, tripods and tetrapods) of Sn-doped nanocrystals in CCl4. The nominal doping concentration is the same (8%) for all the samples and the real doping concentrations are 7.9%, 8.6%, 8.4%, and 8.3%, respectively, determined by ICP-AES techniques. Reproduced from ref. 53 with permission from RSC, copyright 2017. |
Fig. 10 Optical properties of Ce:In2O3 nanocrystals. (a) FTIR liquid cell spectra of Ce:In2O3 and Sn:In2O3 nanocrystals dispersed in tetrachloroethylene showing narrow and tunable MIR LSPR of Ce:In2O3. (b) Tauc plots showing systematic increase in Ce:In2O3 optical band gap with Ce content, consistent with a Burstein–Moss shift. (c) LSPR of 5.2% Ce-doped In2O3 dispersed in nonpolar solvents with different refractive indices. Inset: LSPR peak wavelength versus refractive index. Reproduced from ref. 50 with permission from ACS, copyright 2016. |
Furthermore, in another interesting piece of work by Milliron et al.50 cerium (Ce)-doped In2O3-based NCs were proposed. To synthesize Ce:In2O3 NCs, indium acetylacetonate, cerium precursor, and OLA were mixed in a three-neck round-bottom flask, connected to a Schlenk line and heated to 250 °C for 2 h in an inert environment. Fig. 11 represents the optical characterization of Ce:In2O3 NCs with the different doping contents of Ce. As shown in Fig. 11a, the Ce:In2O3 NCs exhibit a narrow LSPR peak compared to ITO NCs with the peak shifted to higher energy with an increase in the Ce content. Furthermore, the band gap of the NCs was also found to increase with an increase in Ce doping. Further, when dispersions of NCs were made in different nonpolar solvents (with increasing refractive index), a redshift in the LSPR peak was observed (see Fig. 11c). Additionally, Ce:In2O3 NCs were found to exhibit an electron mobility value of 33 cm2 V−1 s−1, higher than that of ITO NCs, making them ideal for transparent conducting applications. Furthermore, S. H. Cho et al.54 synthesized fluorine (F), Sn co-doped In2O3 NCs with the hot-injection method. The co-doped NCs exhibit LSPR characteristics in the NIR region.
Fig. 11 (a) Optical extinction and (b) XPS depth profiling versus doping for the doping series. The dotted black line in panel (b) shows the expected Sn/(In + Sn) ratio for a uniform doping profile. Reproduced from ref. 51 with permission from ACS, copyright 2014. |
Furthermore, molybdenum (Mo) and tungsten (W) were also incorporated into In2O3 and showed LSPR in the mid-IR region.55 To synthesize Mo and WO doped In2O3 NCs (IMO and IWO), the metal/dopant precursors were mixed with OLA and heated at 250 °C and 300 °C, respectively. Fig. 12 shows the LSPR absorption spectra and Tauc plots of IMO and IWO NCs. Clearly, both NCs exhibit LSPR in the mid-IR region with the peak shifted to higher energy with an increase in the doping content of Mo and W. Furthermore, the band gap also increases with an increase in doping due to the Burstein–Moss effect. Similarly, antimony (Sb) and titanium (Ti) doped In2O3 NCs exhibit LSPR in the mid-IR region.56 At a similar doping level of Sb and Ti, the LSPR of Ti-doped NCs was found to be at lower energies and possessed smaller bandwidths compared to Sb-doped In2O3 NCs. This indicates the lower density of free electrons in Ti-doped In2O3 NCs. In an impressive study, the synthesis of zirconia (Zr)-doped In2O3 NCs via a hot-injection method was described for the first time.52 By calculating the quality factor (Q-factor) of LSPR, which is defined as the ratio of LSPR peak energy to its line width, the authors represented the dopant selection criteria. It was found that for high LSPR energy, a stable oxidation state and deeper donor state in the conduction band of the host are required. While for small LSPR, the full width at half maximum (FWHM) requires a higher charge/radius ratio and lower electronegativity of the dopant cation corresponding to the host cation. In this regard, Zr is found to be an ideal aliovalent dopant for In2O3 as it exhibits the highest Q-factor compared to any other plasmonic material reported in the literature so far. The FTIR spectra of Zr-doped In2O3 NCs with different doping contents and the corresponding Q-values are shown in Fig. 13. Clearly, the NCs showed LSPR fingerprints in the mid-IR region.
Fig. 12 (a) LSPR absorption spectra of IMO NCs with different doping concentrations, as indicated in the graph. (b) Tauc plots for IMO NCs from panel (a) used to determine optical band gaps. (c) LSPR absorption spectra of IWO NCs with different doping concentrations, as indicated in the graph. (d) Tauc plots for IWO NCs from panel (c) used to determine optical band gaps. Reproduced from ref. 55 with permission from ACS, copyright 2019. |
Fig. 13 Synthesis of Al-doped ZnO NCs. (a) UV-vis-NIR spectra of ZnO NCs doped with different amounts of Al. The inset shows the respective Tauc plots. (b) Charge-carrier concentration evaluated from the LSPR frequency and nominal vs. real (from EDX) Al concentration for ZnO NCs doped with different amounts of aluminum. Reproduced from ref. 57 with permission from ACS, copyright 2019. |
P. Wainer et al.57 synthesized Al-doped ZnO NCs with continuous growth methods. In a typical synthesis, the solution of metal precursor and dopant was first prepared in oleic acid (OA) and oleylamine (OLA), which was then slowly injected (3 mL min−1) into preheated oleyl alcohol. Fig. 14a shows the UV-vis-NIR spectra (the inset indicates the band gap) of pristine and Al-doped ZnO (AZO) NCs with different dopant percentages (AZO5: 5%Al, AZO10: 10%Al and AZO: 20%Al). Clearly, the AZO NCs exhibit LSPR in the NIR region whose intensity was found to increase with an increase in doping concentration. Additionally, the band gap is also found to increase with dopant concentration due to the Burstein–Moss effect. Furthermore, a carrier concentration up to 1020 cm−3 was achieved with the highest doping level of aluminium (see Fig. 14b). Indeed, the authors were able to incorporate 40% of Al into ZnO NCs. In another interesting study, ZnO NCs doped with In, Ga and Al were prepared by a non-injection method (heat-up).60 Initially, precursors (metal and dopant), surfactant and solvent were mixed together in a nitrogen atmosphere at 100–140 °C and then the temperature was gradually increased to 250 °C at a rate of ∼4 °C min−1, leading to the formation of NCs. In Fig. 15, the surface morphologies of ZnO, AZO, Ga-doped ZnO (GZO) and In-doped ZnO (IZO) NCs along with their size distributions are shown. As can be seen from the TEM images, NCs seemed to exhibit both spherical and elongated shapes (and also a few rod-like ones). The sizes of ZnO, AZO, GZO and IZO were found to be 11.2 ± 2.1 nm, 27.1 ± 6.0, 17.5 ± 3.1, and 13.4 ± 2.4 nm, respectively. Furthermore, optical characterization (UV-vis-NIR and FTIR) of all the NCs along with a photograph of the stock solution and their XRD patterns are shown in Fig. 16. Apart from undoped ZnO NCs, all the doped NCs exhibit LSPR in the NIR region. The FTIR study reveals that the LSPR of AZO, GZO, and IZO showed peak values at 7.5, 5, and 3 μm. According to Drude–Lorentz theory, the frequency of LSPR resonance can be related to the charge-carrier density (n) by the following equation:
n = ω2mee0(ε∞ + 2εm)/e2 |
Fig. 14 Optical extinction spectra of different Zr:In2O3 NCs displaying narrow and symmetric LSPR bands increasing in energy with an increase in Zr doping. Spectra were taken by FTIR of NCs dispersed in tetrachloroethylene. Reproduced from ref. 52 with permission from ACS, copyright 2019. |
Fig. 15 Electron microscopy characterization of ZnO-based NCs. (A) TEM images (the scale bar is the same in all TEM images). (B) SEM images (the scale bar is the same in all SEM images). (C) Histograms of size distribution evaluated from TEM images. Reproduced from ref. 60 with permission from the authors: E. Della Gaspera, and J. J. Jasienia, ACS copyright 2014. |
Fig. 16 (A) Optical absorption spectra of equimolar solutions of ZnO-based NCs in TCE. (B) FTIR spectra of the same colloidal solutions. (C) Photograph of the concentrated stock solutions (absorption spectra are obtained by diluting the stock solutions ∼50 times). (D) XRD patterns of the dried powders (the predicted diffraction peaks for bulk wurtzite ZnO are displayed at the bottom). Reproduced from ref. 60 with permission from the authors: E. Della Gaspera, and J. J. Jasienia, ACS copyright 2014. |
Fig. 17 Low- and high-resolution TEM images of AZO NCs. (A)–(C) AZO NCs of different sizes were obtained by injecting precursor solutions containing 0.2 mmol of Al(acac)3 at 230, 240, and 260 °C, respectively. (D) HRTEM image of a pseudospherical AZO NC oriented along the [011] zone axis and the corresponding fast Fourier transform (FFT) in the inset indicating the hexagonal structure of the wurtzite. The lattice fringes correspond to spacings of 2.42 and 2.79 Å derived from FFT which match well the d spacing of the (101) (d101ZnO = 2.47 Å) and (100) planes (d100ZnO = 2.81 Å) of wurtzite ZnO. (E) HRTEM image of a bullet-shaped AZO NC oriented along the [110] zone axis and the corresponding FFT in the inset. The lattice fringes correspond to 2.79 and 2.58 Å, derived from FFT, consistent with the (100) and the (001) (d001ZnO = 2.60 Å) planes, respectively, of wurtzite ZnO. (F) Electron diffraction of AZO NCs with the expected wurtzite pattern indicated in the lower left. Reproduced from ref. 9 with permission from ACS, copyright 2011. |
Fig. 18 (a) Optical absorption spectra of pure ZnO and doped Zn1−xGaxO nanocrystals in the vis-NIR region. The inset depicts the band-gap absorption of the samples. (b) FTIR spectra of doped samples showing the plasmonic NIR absorption. Additional sharp peaks (asterisks) arise from the organic ligand oleylamine absorbed on the nanocrystal surface. Blue and purple asterisks represent N–H stretching and symmetric/asymmetric stretching vibration of long hydrocarbon chains, respectively. The black dotted line and the red vertical dotted line are guiding lines for the shifting of plasmonic absorption. Reproduced from ref. 61 with permission from RSC, copyright 2015. |
Fig. 19 (a) Optical absorption spectra of equimolar colloidal solutions of ZnO:Ge in tetrachloroethylene (TCE). The inset shows a digital photograph of the prepared colloidal solutions. (b) Tauc plots (exponent = 2, direct band gap) of the ZnO:Ge colloidal solutions. The dashed lines are the linear fits used to identify the band gap. (c) Optical band gap and real Ge/Zn amount evaluated from XRF as a function of the nominal Ge/Zn ratio. Reproduced from ref. 62 with permission from RSC, copyright 2015. |
Fig. 20 (a) UV-vis-NIR absorption spectra of WO2.83 nanorods in N-methylpyrrolidone upon heating at 175 °C in air for 0, 2, and 6 min. (b) XRD patterns of WO2.83 nanorods in N-methylpyrrolidone (top) before and (middle) after heating at 175 °C for 6 min in air and (bottom) the reference pattern for WO2.83. Reproduced from ref. 15 with permission from ACS, copyright 2012. |
Fig. 21 High-resolution TEM images of (a) WO2.72 rods and CsxWO3 (b) hexagonal prism, (c) truncated cube, and (d) pseudospheres. All scale bars are 5 nm. Reproduced from ref. 69 with permission from ACS, copyright 2014. |
Fig. 22 UV-vis-NIR absorbance of WO3−x nanocrystals – LSPRs in different protic polar solvents. Reproduced from ref. 70 with permission from RSC, copyright 2016. |
Fig. 23 TEM images of octahedral ICO nanocrystals produced at 300 °C using (a) 4 mmol and (b) 3 mmol OLAC and (c) SEM image of the sample shown in b. TEM image of spherical nanocrystals produced at reflux using (d) 5 mmol and (e) 3 mmol OLAC. (f) The unit cell of rock-salt type indium-doped cadmium oxide (ICO). Influence of Shape on the Surface Plasmon Resonance of Tungsten Bronze Nanocrystals. Reproduced from ref. 71 with permission from ACS, copyright 2013. |
Fig. 24 (a) Solution-phase spectra of ICO nanocrystals dispersed in CCl4 for five levels of % atomic doping of In. The fwhm or Γ is indicated for the 16.2% doped sample. (b) Plots of (αhν)2vs. photon energy (eV) for five samples of spherical ICO nanocrystals. Open circles are measured data, dotted lines are linear fits, and the legend shows the extracted direct band-gap energies. Reproduced from ref. 71 with permission from ACS, copyright 2013. |
Fig. 25 (a) Normalized extinction spectra of size controlled CdO NCs synthesized with different HMDS/Cd ratios. (b) Extinction spectra of CdO NCs (8.5 ± 1.2 nm) dispersed in different solvents. (c) Plot of LSPR peak wavelength versus the refractive index of solvent. CCl4: carbon tetrachloride, TCE: tetrachloroethylene, CS2: carbon disulfide. Reproduced from ref. 73 with permission from ACS, copyright 2020. |
Furthermore, fluorine, In co-doped CdO (FICO) NCs were synthesized via the heat-up method.74Fig. 26(a–c) show the TEM images, UV-vis-NIR spectra and Tauc plots of FICO NCs. As can be seen from Fig. 26a, the FICO NCs are found to be spherical in shape. At all the doping concentrations, sharp LSPR peaks were observed, which shifted to lower wavelength as the doping concentration increased (Fig. 26b). Furthermore, the band gap of FICO NCs also increased with an increase in the In doping level underlying the Burstein–Moss effect.
Fig. 26 (a) Transmission electron microscopy images of FICO 3% (diameter 20.2 ± 1.8 nm). (b) Normalized absorption spectra of FICO NC samples with different doping levels. (c) Plots of (αhν)2vs. photon energy (hν) for the FICO NC samples shown in (b). Reproduced from ref. 74 with permission from ACS, copyright 2019. |
Degenerately doped MOX NCs can be seen as IR detecting media because of the possibility of tuning the LSPR from the deep MIR to the NIR region by optimizing the carrier concentration using different dopants. Furthermore, the availability of scalable synthesis methods like heat-up or continuous growth makes it favourable over 2D materials. In an interesting piece of work, Qu et al.89 explored the potential of ITO NCs for IR photodetector applications. Due to the weak photo-signal that is linked with the poor charge transport in NCs (a similar issue to narrow-band-gap QDs) and weak extraction of LSPR-assisted hot-electrons, very poor photodetector performance was observed. To overcome the obstacle of hot-electron extraction, a heterostructure of MOX NCs (ITO) and MoS2 has recently been proposed, which we have already discussed in Section 3. However, when making optoelectronic devices like photodetectors, charge transport within the active material and their collection at the respective electrodes defines the efficiency of the devices. In this regard, the heterojunction between narrow-band-gap PbS QDs and ZnO nanowires (NWs) was proven to be effective,81,87 in which the QDs act as an NIR sensitizer and NWs provide the conduction path to electrons. Indeed, the charge transport in NWs is believed to occur at a speed several orders of magnitude faster than in nanoparticles like QDs or NCs, primarily attributed to the minimized scattering effects resulting from the limited presence of grain boundaries.90 Additionally, due to the quantum confinement effect, NWs provide unidirectional and better control of charge transport, leading to high charge-carrier mobility.90 Hence, the heterojunction of NCs with 2D materials, nanowires etc. can been seen as step forward to fabricate the future generation of IR photodetectors based on degenerately doped MOX NCs.
Furthermore, nanostructured MOXs have been explored and proven to be highly efficient for chemical sensing applications.91–98 However, recently, the development of self-powered sensors for real-time environmental and health monitoring has gained momentum, driven by the urgency of the energy crisis, environmental pollution, and climate change.23 Harnessing energy from sunlight is always an ideal and dependable choice due to its cleanliness, safety, and the vast energy reserves Earth receives from the sun. A sensor that harnesses energy from sunlight is known as a photovoltaic (PV) self-powered sensor.79 However, the current state-of-the-art for PV self-powered sensors, whether utilizing sunlight or other activation sources, is still far from reaching the essential “3S of a sensor”: sensitivity, selectivity, and stability.22,23,99 In this regard, photoactivated (UV) MOX-based gas sensors have gained significant attention for developing RT or low-power-consuming sensors.22 By fabricating these MOXs in different nanostructure forms and by tuning their band gap, photoactivation with visible light has also been achieved.23 It was observed that by designing suitable device structures, these photoactivated MOX sensors are able to achieve self-sustaining operation using the photovoltaic (PV) effect.100–102 To further extend light harvesting to the IR region, degenerately doped MOX NCs can be employed as an active sensing platform. Sturaro et al.103 proposed gallium-doped zinc oxide (GZO) NC based optical (plasmonic) and chemiresistive sensors for the detection of hydrogen (H2) and nitrogen dioxide (NO2). To realize a sensing device, an NC thin film was deposited by spin-coating onto an SiO2 substrate. The sensing measurements were performed at 80 and 200 °C. In the chemiresistive gas sensing of these NCs, the authors observed some response at room-temperature under illumination by blue light and the response increased with an increase in the operating temperature of the sensor. These were preliminary investigations, as many important factors, such as sensor selectivity, sensitivity and stability, need to be explored. However, it indeed gives us the idea and possibility to use degenerately doped MOX NCs to build PV self-powered sensors that harvest energy from UV-vis-IR radiation. In this sense, the heterostructure of NCs with MOX NWs can be effective. The reason behind this argument is that a chemiresistive sensor based on MOX NWs is already an established sensing platform and it showed fast response dynamics, selectivity, and stability due to the high surface-to-volume ratio, well-defined crystal orientation and controlled unidirectional electrical properties.94,104,105
Hence, by carefully manipulating the plasmonic properties of degenerately doped MOX NCs and using a suitable device configuration, a future generation of IR photodetectors and PV self-powered chemical sensors can be developed.
This journal is © The Royal Society of Chemistry 2024 |