aInstituto de Ciencia Molecular (ICMol), Universitat de Valencia, Catedrático José Beltrán Martínez n° 2, 46980 Paterna, Valencia, Spain. E-mail: isabel.abanades@uv.es; francisco.c.garcia@uv.es
bWestCHEM School of Chemistry, University of Glasgow, Joseph Black Building, University Avenue, Glasgow G12 8QQ, UK
First published on 18th May 2022
The influence of composition and textural characteristics of a family of ultra-small isoreticular UiO-type metal–organic frameworks (MOFs) with different functionalized and extended linkers on their catalytic performance is evaluated. Two direct amide bond formations across four different substrates (benzylamine + phenylacetic acid and aniline + formic acid) are employed as proof-of-concept reactions to test the activity of the Zr-MOF nanoparticles. The reaction rates of amide bond formation are evaluated against physico-chemical properties such as crystallinity, porosity, particle size or linker functionality, alongside the Lewis acid and hydrophobic properties of the MOFs, in order to gain insights into the catalytic mechanism and optimal properties for its enhancement.
Thus, the design of a catalyst able to favour the processes at lower temperatures, under solvent-free conditions, and to direct it towards the formation of the N–C bond between the amine and carboxylic acid, is needed. Different homogeneous and heterogeneous catalysts are reported for such endeavours, such as Brønsted (sulfonic acids, HPW, Si-OH, etc.) or Lewis (Ti, Zr, Nb, Al, Zn, etc.) acids. In this sense, heterogeneous catalysts are preferred over homogeneous ones since their recovery and recycling is facilitated. Particularly, porous solids are a fundamental class of heterogeneous catalysts, given their high surface areas and pore volumes, ability to facilitate the dispersion of active sites, and the enhanced diffusion of substrates and products. This is indicated by pioneering interest in the application of clays,7,8 zeolites9 or mesoporous silica10 to promote direct amidation reactions during the last decades.
Recently, metal–organic frameworks (MOFs) have appeared as a novel class of hybrid metal–organic porous material with a crystalline and highly tailorable structure, and they are being increasingly applied as heterogeneous catalysts.11–16 In this sense, MOFs offer the possibility of immobilizing acid sites in the nodes of porous frameworks that allows well-defined and accessible active sites in the solid matrix.17–21 Among all the metals employed in the synthesis of robust and active MOF-based catalysts, Zr(IV) MOFs such as the UiO family or MOF-808, which contain Zr6O4(OH)4(RCO2)12 clusters, have been widely applied for the activation of carbonyls or other oxo-functions due to the presence of highly oxophilic coordinatively unsaturated sites (CUS).22–25 These MOFs are also the preferred systems in acid-catalyzed direct amidation reactions between carboxylic acids and amines.26–28 On the one hand, Timofeeva et al. considered either the sulphated cluster or the pore size – in the case of sulfonated MOF-808 or UiO-66, respectively27 – as key factors for the formylation of aniline under solvent-free/MeOH room temperature conditions (see Scheme 1a).
Scheme 1 (a) Formylation of aniline, and (b) reaction between phenylamine and phenylacetic acid catalysed by the CUSs of the Zr-MOFs MOF-808 and UiO-66.27,28 |
MOF-808 outperformed pristine UiO-66 when using methanol as solvent (78% vs. <1% yield, respectively, at 35 °C for 90 min), although no further information on the performance of UiO-66 under solvent-free conditions was provided. On the other hand, UiO-66 was also recently employed as a heterogeneous catalyst by de Azambuja, Parac-Vogt and co-workers for the reaction between benzylamine and phenylacetic acid (see Scheme 1b).28
Zr-dicarboxylate MOFs of the UiO-66 isoreticular series (see Fig. 1) are commonly investigated in catalysis due to the fact that the Zr6O4(OH)4 secondary building unit (SBU) can be maintained while linkers with slight microscopic variations in the composition, such as the presence of substitutions on the aromatic ring, can be incorporated, resulting in significant changes in the macroscopic properties of the final MOF, such as the hydrophobicity, pore size or catalytic activity.22 Indeed, employing different linkers allows fine-tuning the electronic and steric properties of the metal-oxo clusters in this highly robust Zr-UiO MOF platform.22,23
However, in the context of direct amide bond formation, the use of Zr-dicarboxylate MOFs and derivatives (i) under solvent-free mild conditions, (ii) with different linker functionality and size and (iii) in the form of ultra-small nanoparticles have been less explored (especially the last point) in the assessment of catalytic performance. Thus, the differences in amidation activity of isoreticular MOFs containing similar Zr-oxo clusters with different types of linkers need to be better understood.
Herein we report the synthesis, characterization and catalytic activity of ultra-small Zr-dicarboxylate MOF nanoparticles made with linkers of varied functionality and size (BDC, BDC-NH2, BDC-NO2, BDC-OH, NDC and BPDC), as represented in Fig. 1, in order to tune their physicochemical properties (i.e. porosity, organic group composition) and thus chemical reactivity towards carboxylic acid (i.e. phenylacetic acid and formic acid) and amine (i.e. aniline and benzylamine) functions. In this work, we aim to apply Zr-MOF ultra-small nanoparticles designed with different functionalities as catalysts for direct amide bond formation and to study the effect of the linker functionality and size on their catalytic activity.
For reaction B, 20 mg of phenylacetic acid (0.15 mmol) and 20 μL of benzylamine (0.19 mmol) were dissolved in 200 μL of methanol-d4 and added to a vial containing 10 mg of MOF. The mixture was heated at 60 °C for 24 h under stirring at 300 rpm. Sample aliquots were taken after this time and analysed as described for the formylation reaction.
Fig. 2 Characterization of the Zr-MOFs by (a) PXRD together with simulated UiO-66 pattern with FWH 0.7, (b) N2 adsorption and desorption isotherms and (c) TGA. |
N2 physisorption measurements of the samples, represented in Fig. 2b show that these small nanoparticles exhibit mesoporosity, together with a decrease in microporosity (see Fig. S21–S30†). This is in great agreement with reports showing that drastically reducing the particle size results in an increase in the mesoporosity and a decrease in the microporosity.30 In particular, the Zr-BPDC sample exhibits the highest porosity (with a surface area of 2006 m2 g−1), while the Zr-BDC-OH, Zr-BDC-NO2 and Zr-BDC-NH2 are the less porous ones (452, 484 and 593 m2 g−1, respectively). However, the nanoparticles exhibit remarkably high pore volumes coming both from the induced mesoporosity (below P/P0 = 0.9) and interparticle adsorption (above P/P0 = 0.9), with twice the reported pore volume of pristine samples.11,23,30
Fourier transform infrared (FTIR) spectra of the samples were performed in order to confirm the presence of the functional groups in the benzene ring of the linker (i.e. NH2, NO2, OH), as indicated in Fig. S31 and S32.† The FTIR spectrum of the Zr-NDC sample indicates the absence of physisorbed water, suggesting high hydrophobicity, when compared with the rest of the samples. Additional information on the composition and defectivity (experimental linker-to metal ratio) of ultra-small nanoparticles can be extracted from the 1H-NMR spectra of digested samples (see Table S3†) and thermogravimetric analysis of the MOFs (see Tables S4 and S5, and Fig. S33 and S34†). The molar ratio of modulator per linker (i.e. acetic and formic acid) oscillates between 0.14–1.1 for acetic acid, and 0.08–0.75 in the case of formic acid, despite the latter originating from the decomposition of DMF during synthesis, and the former being added to synthesis (ca. 18 equivalents) possibly due to the higher acidity of formic acid. The presence of formate defects in the catalysts is particularly relevant to aniline formylation, given formic acid is a reagent in this process. Although TGA cannot differentiate between the type of defect (i.e. missing linkers or missing clusters), it provides information about the linker to metal ratio.31 The linker to metal ratio (L/Zr = 1 for the pristine materials) varied between 0.77 and 0.98, which corresponds to a molar percent of linker deficiency of 1.1% (for Zr-BDC-NO2) and 22.9% (for Zr-NDC).31 We have summarized the above-mentioned information about the samples’ textural properties and linker/modulator incorporation – also described in the ESI† – in Table 1.
Zr-MOF | S area/m2 g−1 | Pore volume/cm3 g−1 | NP size/nm | %HCOOHa | L/Zr | %MLb |
---|---|---|---|---|---|---|
a Formic acid incorporated in the MOF from solvent breakdown. b Molar percent of linker deficiency (1-L/Zr × 100) | ||||||
Zr-BDC | 894 | 0.74 | 13 ± 4 | 0.08 | 0.973 | 2.7 |
Zr-BDC-OH | 452 | 0.49 | 15 ± 3 | 0.75 | 0.810 | 19.0 |
Zr-BDC-NO2 | 484 | 0.53 | 28 ± 4 | 0.54 | 0.989 | 1.1 |
Zr-BDC-NH2 | 593 | 0.69 | 18 ± 2 | 0.32 | 0.781 | 21.9 |
Zr-NDC | 769 | 0.94 | 39 ± 6 | 0.15 | 0.771 | 22.9 |
Zr-BPDC | 2006 | 2.33 | 39 ± 7 | 0.40 | 0.984 | 1.6 |
Although exhibiting a moderate activity, both samples were slightly more active (initial reaction rate r0 = 3.0 mmol h−1) with respect to the blank reaction (r0 = 2.3 mmol h−1). The initial rate of aniline formylation in the presence of the non-functionalized Zr-BDC, Zr-BPDC and Zr-NDC is similar to the blank reaction (see bars 1 and 4–7 in Fig. 3a). The yields obtained (Table S7†) are in line with those reported in the literature in the case of UiO-66 (<5% yield) under similar reaction conditions.27
We have performed reusability of one of the best performing MOFs (Zr-BDC-NH2) for 3 consecutive cycles, each of them with a reaction time of 30 minutes (see Fig. S42 and Table S8†). A minor decrease in product yield is observed (from 72% to 65%) likely due to the loss of part of the MOF powder during the centrifugation/re-dispersion cycles of the reusability testing. Both the presence of only traces of Zr (<0.51 wt% of the fresh MOF, assessed by ICP measurements) and the absence of ligand in the 1H-NMR spectra suggest minimum leaching of metal and linker from the MOF to the reaction medium after the three catalytic cycles. The homogeneous Zr(IV) loading corresponding to this amount of leaching (<0.1 wt% with respect to aniline) has a negligible catalytic effect according to a previous report where 2–10 mol% ZrCl4 is required as the catalyst of direct amidation of carboxylic acids with amines.6 To assess the stability of the ultra-small Zr-MOF nanoparticles under these reaction conditions, we have measured their PXRD patterns after the reaction and compared them with those of the “as-prepared” samples (see Fig. S43–S48†). In general, the diffractograms show no major changes in the peaks’ positions and width, which is indicative of the maintenance of their crystalline structure and particle size, apart from a minor crystallinity decrease for Zr-BPDC and Zr-NDC (see Fig. S47 and S48†). To further confirm the importance of the ultra-small nanoparticle size on the catalytic activity we have compared the activity of Zr-BDC-NH2 with that of standard Zr-BDC-NH2 (see Fig. S49 and S50† and Table S9†). While the nanosized (ca. 20 nm) MOF surpasses the activity of the blank reaction (34% yield), the standard Zr-BDC-NH2 MOF (ca. 440 nm) gives a similar conversion to the blank autocatalytic reaction (22% yield) after 1 h.
On the other hand, we attempted the synthesis of N-benzyl-2-phenylacetamide by reacting phenylacetic acid and benzylamine in the presence of the Zr-MOF samples (5 mol%). As for the aniline formylation, the 1H-NMR spectra of the reactions, calculated yields and rates are presented in Fig. S51† and Table S10,† respectively. Compared to the blank reaction, all Zr-MOF samples catalyze the amidation reaction between phenylacetic acid and benzylamine in deuterated methanol at 60 °C for 24 h, resulting in yields similar to what was recently published for UiO-66 (ca. 15% yield for ca. 5 mol% MOF loading). Fig. 3b shows that hydrophobic MOF materials such as the Zr-BDC-NO2 (r0 = 0.94 μmol h−1) or Zr-NDC (r0 = 0.62 μmol h−1) present a higher activity than parent Zr-BDC (0.56 μmol h−1) or the blank reaction (r0 = 0.25 μmol h−1). The yields of N-benzyl-2-phenylacetamide using Zr-BDC-NO2 (see Table S10†) are comparable to the reported values for UiO-66 (10% mol) in ethanol as solvent at 80 °C (ca. 15%). However, the conditions reported here are milder in terms of temperature (60 °C) and MOF loading (5 mol%), which is half of the loading reported.28 A higher yield can be obtained when the reaction time is increased to 72 h, obtaining a ca. 37% yield with the Zr-NDC catalyst, while no product is detected in the absence of a catalyst (see Fig. S52†). In addition, the catalyst shows good reusability with a minor decrease in catalytic activity that arises from loss of the powder during centrifugation/redispersion cycles, whereas the uncatalyzed reaction shows no conversion at any point (see Fig S53† and Table S11†).
On the one hand, the surface area (and the related pore volume and % mesoporosity) of the samples does not have a clear influence on the rate of aniline formylation (see blue circles in Fig. 4a). In fact, the formylation rate is lower in the presence of the large surface area materials Zr-NDC and Zr-BPDC, compared with the higher rate achieved with low surface area materials Zr-BDC-NO2 or Zr-BDC-NH2. This suggests that the reaction between aniline and formic acid – substrates with small molecular sizes – is not controlled by diffusion and that the formylation is the rate-determining step. In contrast, a linear trend between these two variables (reaction rate and surface area) can be observed in the reaction between bulkier phenylacetic acid and benzylamine (see red squares in Fig. 4a), in the presence of Zr-BDC-OH (452 m2 g−1), Zr-BDC-NH2 (593 m2 g−1), Zr-BDC (894 m2 g−1) and Zr-NDC (769 m2 g−1). The unexpected high and low reaction rates obtained with Zr-BDC-NO2 (484 m2 g−1) and Zr-BPDC (2006 m2 g−1), respectively, may be a consequence of two facts: (i) the stronger Lewis acidity of Zr-BDC-NO2 (with electron-withdrawing -NO2 groups); or (ii) the lower stability of Zr-BPDC (due to rotation of the biphenyl group), which is further suggested by the poorer crystallinity, as assessed by PXRD, of the spent material. In the case of Zr-BDC-OH and Zr-BDC-NH2, the presence of electron-donating groups and thus weaker Lewis acidity of the Zr sites might also decrease their catalytic activity in addition to the surface area effect.
On the other hand, the size of the ultra-small Zr-MOF nanoparticles presents an optimal value of ca. 20–25 nm to increase the reaction rate of amide bond formation in the two examples studied here (see Fig. 4b). This is especially clear in the case of aniline formylation, where Zr-BDC-NO2 (ca. 28 nm) and Zr-BDC-NH2 (ca. 18 nm) are the most active catalysts. Lower (Zr-BDC and Zr-BDC-OH) and higher (Zr-NDC and Zr-BPDC) nanoparticle sizes are related to lower reaction rates. Despite the lower sizes of Zr-BDC and Zr-BDC-OH nanoparticles (13 and 15 nm, respectively) increasing the availability of catalytic Zr6 sites on particle external surfaces, the larger Zr-BDC-NO2 nanoparticles increase the rate of both reactions to a higher extent. As proposed in the discussion of the surface area (as well as in literature),22,23 the stronger acidity and hydrophobicity of Zr-BDC-NO2 may be the keys to its differential behaviour.
Regarding the sample composition and potential defectivity, two variables were studied: the molar percent of linker deficiency (obtained from TGA) and the incorporation of formate ions (obtained from 1H-NMR spectroscopy) in the MOFs, which although came from the decomposition of DMF during synthesis are more significantly incorporated than the added acetate ions in some cases. The molar percent of linker deficiency in Zr-BDC, Zr-BDC-NO2 and Zr-BPDC is significantly lower (1–3%) than in Zr-BDC-OH, Zr-BDC-NH2 and Zr-NDC (19–23%). However, no clear dependence of the reaction rate on the missing linker density can be established at this point (see Fig. 4c). The relationship between the formylation rate and the %HCOOH is plotted in Fig. 4d, suggesting that moderate concentrations of HCOOH in the MOF (ca. 0.5 FA per linker) are beneficial for their catalytic activity in the formylation of aniline; adsorbed formate intermediates have been proposed for other solid acid catalysts of amide bond formations.32 However, larger amounts of this modulator are detrimental for the MOF catalytic activity, probably due to extensive coordination to the CUSs at the Zr-oxo clusters, thus decreasing the number of active sites.22 It should be noted that the additional formate introduced into the reactions by the catalyst is minimal when comparing the 5 mol% catalyst loading to the 5-fold excess of formic acid used.
Catalyst | Temperature/°C | Solvent | HCOOH: aniline | Yield (reaction time) | Activity/mmol h−1 gcatalyst−1 | Ref. |
---|---|---|---|---|---|---|
Zr-BDC-NH2 | 35 | Solvent-free | 5 | 72% (0.5 h) | 300 | This work |
MOF-808 | 35 | Solvent-free | 2 | 95% (0.3 h) | 864 | 27 |
UiO-66 | 35 | Methanol | 1.2 | <1 (1.5 h) | <1 | 27 |
ZnO | 25 | Solvent-free | 4 | 70% (0.16 h) | 4.5 | 33 |
Al2O3 | 40 | Solvent-free | 3 | 98% (0.08 h) | 2147 | 34 |
For the synthesis of N-benzyl-2-phenylacetamide from the reaction between phenylacetic acid and benzylamine, Francisco de Azambuja et al. obtained a 14% yield of amide product after 24 h in the presence of UiO-66 (10 mol%) in ethanol at 80 °C.28 This is associated with a reaction rate of ca. 35 μmol h−1 gMOF−1, a smaller value than the 94 μmol h−1 gMOF−1 obtained with Zr-BDC-NO2 under milder conditions (methanol-d at 60 °C) with 5 mol% of catalyst.
Therefore, we propose the dissociative adsorption of the carboxylic acid at the Zr-oxo cluster due to the high oxophilicity of these SBUs, as a previous step to the nucleophilic attack of the amine and water elimination (see Scheme 2). In this sense, little information has been offered on the process of water elimination (to form the amide bond) during the reaction mechanism from the point of view of the materials’ properties, such as the hydrophobicity of the material. We propose that the hydrophobicity of the MOF increases its catalytic activity. This is indicated by the low water content of the Zr-NDC sample, evident in its FTIR spectrum (Fig. S31†), which contains a naphthalene moiety with respect to benzene or biphenyl-based MOFs, resulting in high catalytic activity in the synthesis of N-benzyl-2-phenylacetamide. In contrast, more hydrophilic H-bond forming OH and NH2-functionalized linkers in Zr-BDC-OH and Zr-BDC-NH2 might be detrimental to the water desorption step, in line with their poor activity in the synthesis of N-benzyl-2-phenylacetamide. Besides the hydrophobicity, the high activity of Zr-BDC-NO2 might also be related to its stronger Lewis acidity and hydrophobicity based on our previous results.22,23,36
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2dt00369d |
This journal is © The Royal Society of Chemistry 2022 |