aCollege of Polymer Science and Engineering, State Key Laboratory of Polymer Materials Engineering, Sichuan University, Chengdu 610065, China. E-mail: dingcm@scu.edu.cn; jianshu_li@scu.edu.cn
bDepartment of Pain Management, West China Hospital, Sichuan University, No. 37, GuoXue Xiang, Chengdu 610041, China
cDepartment of Orthopedics, People's Hospital of Deyang City, No. 173, Taishan North Road, Deyang 618000, China
dState Key Laboratory of Oral Diseases, West China Hospital of Stomatology, Sichuan University, Chengdu 610041, China
eCAS Key Laboratory of Bio-inspired Materials and Interfacial Science, Technical Institute of Physics and Chemistry, Beijing 100190, China
fMed-X Center for Materials, Sichuan University, 610041, China
First published on 10th September 2021
Inspired by the intricate extracellular matrix (ECM) of natural cartilage and subchondral bone, a heterogenous bilayer hydrogel scaffold is fabricated. Gelatin methacrylate (GelMA) and acryloyl glucosamine (AGA) serve as the main components in the upper layer, mimicking the chondral ECM. Meanwhile, vinylphosphonic acid (VPA) as a non-collagen protein analogue is incorporated into the bottom layer to induce the in situ biomineralization of calcium phosphate. The two heterogenous layers are effectively sutured together by the inter-diffusion between the upper and bottom layer hydrogels, together with chelation between the calcium ions and alginate added to separate layers. The interfacial bonding between the two different layers was thoroughly investigated via rheological measurements. The incorporation of AGA promotes chondrocytes to produce collagen type II and glycosaminoglycans and upregulates the expression of chondrogenesis-related genes. In addition, the minerals induced by VPA facilitate the osteogenesis of bone marrow mesenchymal stem cells (BMSCs). In vivo evaluation confirms the biocompatibility of the scaffold with minor inflammation and confirms the best repair ability of the bilayer hydrogel. This cell-free, cost-effective and efficient hydrogel shows great potential for osteochondral repair and inspires the design of other tissue-engineering scaffolds.
The physiochemical properties of the scaffold, such as the composition and stiffness, are vital to the cell behaviour and are usually engineered to allow tissue regeneration by the manipulation of the cell fate.13 The intricate ECM of natural cartilage and subchondral bone inspires the choice of materials. For the cartilage layer, chondrocytes are located in the gel-like ECM with the main components of collagen, glycosaminoglycans (GAGs), proteoglycan and water;14 however, for the subchondral layer, aside from collagen, calcium phosphates (CaPs) induced by organic proteins and cells constitute the majority of the ECM.15 In light of this, double-layer hydrogels with the components of collagen (or gelatin), GAGs and CaPs have been technically constructed to simulate the natural ECM.5 Although large efforts have been made, the regeneration of articular cartilage has been far from satisfactory. As a consequence, it is of great significance to discover materials that are beneficial for cartilage repair. Moreover, in particular, the favourable stiffness for chondrogenic and osteogenic differentiation of BMSCs shows a large difference.16 With regard to this, bilayer hydrogels are normally constituted by a soft cartilaginous layer and a stiff subchondral bone layer.17 Nevertheless, it remains a great challenge to realize stable interfacial bonding between two layers that have a different composition and stiffness.
Aiming at the above two problems, we attempt to design heterogenous bilayer hydrogels with a robust interfacial bonding strength and a local environment that is favourable for osteochondral defect repair, especially the restoration of articular cartilage. Glucosamine is a fundamental constituent of GAGs and forms the basic moieties of saccharides. Very recently, our group has found the positive role of these moieties for the chondrogenic differentiation of BMSCs.18 Furthermore, glucosamine also possesses the ability to prevent joint space narrowing19 and can enhance chondrogenesis.20 On the basis of this, it is reasonable to expect the advantageous effect of glucosamine for cartilage regeneration, which is rarely investigated nowadays. Herein, gelatin methacrylate (GelMA) and acryloyl glucosamine (AGA) are incorporated as ECM mimetics of the upper cartilage layer (collagen and glucosamine). Meanwhile, to afford CaPs in the bottom layer, vinylphosphonic acid (VPA), as an NCP analogy, is adopted to induce the biomineralization of CaPs by abundant phosphate groups, as referred to in our previous work.21 The incorporation of CaPs improves the stiffness of the bottom layer of the hydrogel, and is beneficial for bone regeneration. Moreover, the two layers with diverse compositions and mechanical properties were sutured into an intact layer by delicate control of the interdiffusion between the upper and bottom layer hydrogels, together with the chelation between calcium ions and alginate added to the separate layers (Scheme 1). The physicochemical properties of the monomers and hydrogels were investigated. Cell experiments with chondrocytes and BMSCs were conducted on the upper and bottom layers, respectively. Moreover, the repair of osteochondral defects was evaluated in vivo.
Scheme 1 Schematic illustration showing the ECM-inspired double-layer hydrogel for the repair of osteochondral defects. |
For the synthesis of AGA (Fig. 1c), glucosamine (GA, 0.02 mol) was dissolved in 1 M K2CO3 solution (20 mL). Acryloyl chloride (0.024 mol) was added dropwise to the solution at −4 °C for the reaction for 4 hours in the dark; after this, the whole solution was then allowed to evaporate at room temperature for 24 hours to remove the unreacted acryloyl chloride. The as-prepared mixture was dissolved in water, lyophilized and purified using silica column chromatography. Finally, the obtained solution was lyophilized again and stored at −20 °C.
DS = (1 − kmodifiedgelatin/kgelatin) × 100% | (1) |
Meanwhile, GelMA and AGA with different concentrations were dissolved in deionized water (DIW), with the addition of Irgacure 2959 (0.5 wt%) and CaCl2 (100 mM) as the precursor solution of the upper-layer hydrogel. The concentrations of GelMA and AGA were regulated as: G9A1–GelMA (13.5 wt%) and AGA (1.5 wt%), G14A1–GelMA (14 wt%) and AGA (1 wt%), and G19A1–GelMA (14.25 wt%) and AGA (0.75 wt%). After degassing, the solution was poured on the top of the bottom-layer solution, which had been pre-cured for 3, 5 and 7 min. The whole system was then exposed to UV light at the wavelength of 365 nm (1000 W) for 20 min. After curing, the bilayer hydrogels with different sizes were obtained. For the preparation of single-layer hydrogels, the mould was filled with either the upper- or bottom-layer hydrogel precursor solution and cured under the same conditions as for the bilayer hydrogels.
To investigate the effect of interfacial chelation (sodium alginate–Ca2+) on the rheological properties, the upper-, bottom- and double-layer hydrogels were also prepared similarly as above, except that the sodium alginate and CaCl2 were not added.
The obtained hydrogels were initially immersed in PBS at 4 °C for 24 hours to remove unreacted monomers, and then the bottom layers of the hydrogels were immersed in the Ca/P metastable solution at room temperature for 3 hours. The hydrogels were then removed, washed with PBS, and soaked in mSBF solution at 37 °C for 32 hours with the exchange of fresh mSBF every 16 hours. The mineralized hydrogels were rinsed with DIW, cut to the required sizes, and stored at 4 °C before use.
SR = (W1 – W0)/W0 | (2) |
Hydrogels of the same size as for SEM observation were also tested for their mechanical properties using a universal testing machine (HZ-1004, Hengzhun, China). A compressive rate of 0.2 mm min−1 was applied, and the test was terminated once the hydrogel had fractured. Stress–strain curves were obtained and utilized for calculation of the compressive modulus value (normally ∼0–3% strain).
The rheological properties of the hydrogels were characterized at room temperature using an Anton Paar rheometer (MCR 302, Austria). Samples with a diameter of 25 mm and a thickness of 2 mm were placed between the bottom and upper plates of the rheometer. The strain sweep was carried out for the deformation range from 0.1 to 100 at a shear stress of 0.1 N and a frequency of 1 Hz. The frequency sweep was conducted from 0.1 to 100 Hz with a shear deformation of 1%.
BMSCs were isolated from new-born Sprague Dawley (SD) rats (1 week). In brief, bone marrow was collected and cultured in a medium of 90% α-MEM, 10% fetal bovine serum (FBS) and 1% penicillin streptomycin under a 5% CO2 atmosphere at 37 °C. BMSCs were sub-cultured and harvested at passage 3 for the following experiments.
BMSCs were seeded in a 24-well culture plate on the surfaces of bottom layer hydrogels (10 mm in diameter and 1 mm in thickness) at a density of 20000 cells per well. The plates were incubated under 5% CO2 at 37 °C with the culture medium changed every other day. After 3 days of incubation, fluorescence microscopy (Olympus FV1000) was utilized to observe the attachment of the cells. To visualize the adhesion of the cells on the hydrogel, the nuclei of the BMSCs were stained with DAPI, while the F-actin of the cells was stained with rhodamine phalloidin.
Real-time polymerase chain reaction (RT-PCR) was performed to evaluate the gene expression of osteogenic differentiation. In brief, the total RNA was extracted using an RNA isolation kit (Vazyme Biotech Co., Ltd), which was further reverse-transcribed into cDNA using a cDNA synthesis kit (Thermo Fisher Scientific, USA). The cDNA solution was mixed with qCR Master Mix (Bio-Rad) to amplify and evaluate the gene expression of Col-I, osteocalcin (OCN) and runt-related transcription factor 2 (Runx2) using the RT-PCR detection system (CFX96TM, Bio-Rad, USA). The gene expression level of each group was normalized to the control group (BMSCs cultured on a blank culture plate). The primer sequences of each gene are illustrated in Table S2 (ESI†).
To evaluate the protein secretion and gene expression of chondrocytes, cells were seeded in a 12 well culture plate (20 mm in diameter and 1 mm in thickness) on the surfaces of upper layer hydrogels at a density of 50000 cells per well and then cultivated in a humidified atmosphere at 37 °C with 5% CO2. After 7, 14 and 21 days of incubation, chondrocytes were rinsed with PBS, treated with 3 freeze–thaw cycles followed by ultrasonication (SCIENTZ-IID, NingboScientz Biotechnology Co., Ltd, China). The supernatants were collected via centrifugation at 14000 rpm for 20 min, and then examined using a rat Col-II ELISA kit, a rat GAG ELISA kit and a BCA protein assay kit. Notably, the concentrations of Col-II and GAG were normalized using the protein content obtained from the BCA assay kit.
The characterization of the gene expression of the chondrocytes is similar to that of the BMSCs, except that the gene expression of Col- II, AGG and Sox9 was studied. The primer sequences of each gene are illustrated in Table S2 (ESI†).
The synthesis of AGA is completed by the reaction of AG with acryloyl chloride (Fig. 1c).31 The 1H NMR spectrum of AGA (D2O) exhibits distinct peaks at δ ≈ 6.10–6.30 ppm and δ ≈ 5.68–5.74 ppm compared with that of GA (Fig. 1d), which are derived from the vinyl protons of acrylate groups. The other peaks are in good accordance with those reported in the literature: δ(ppm): 6.09–6.31 (Hh, Hi, anti), 5.68–5.74 (Hi, syn), 5.13–5.14 (Ha) and 4.66–4.67 (Ha), 3.35–3.91 (Hb, Hc, Hd, He, and Hf).32 The mass spectrum of AGA further reveals an intense peak at m/z 256.07 (calculated AGA + Na+: 256.08), which accounts for the acylation of the amino group (Fig. 1e). The 1H NMR results together with the mass spectrum confirm the existence of the acrylate group on the AGA molecule.
Meanwhile, VPA was co-polymerized with AAm to act as the bottom-layer scaffold for calcified cartilage. These two layers were sutured together with the assistance of alginate–calcium chelation (see the details in the Experimental section). The direct addition of the precursor solution of the upper hydrogel to that of the bottom hydrogel destroyed the intrinsic integrity of the two separate layers. As a consequence, the precursor solution of the bottom-layer hydrogel was pre-cured using UV irradiation first, followed by the pouring of the upper precursor solution and further UV curing. A pre-curing time of 3, 5 and 7 min was applied to investigate the interfacial bonding between the two layers. The rheological properties of the as-obtained double-layer hydrogels were characterized by subjecting each sample to shear stress. The oscillatory strain sweeps reveal that the storage modulus (G′) maintains its stability and is higher than the loss modulus (G′′) at a low deformation strain, indicating gel-like behaviour under these conditions (Fig. 2a–c).36 When the shear strain was increased above a critical value, G′ decreased to lower than G′′ and the gel state of the hydrogel was disrupted. For hydrogels with pre-curing times of 3, 5 and 7 min, the critical strains are 12.7%, 70.5% and 41.9%, respectively. These results reveal that the irradiation time of 5 min enables the largest resistance to shear deformation. Moreover, the frequency sweeps for each group were recorded (Fig. S1, ESI†). The linear viscoelastic region of G′ at low frequency (∼0.1–5 Hz) denotes the stable mechanical performance of the hydrogel over the long-term (Fig. 2d).37 It should be mentioned that the modulus of the double-layer hydrogel shows a slight increment (14.28 to 14.97 kPa) when the pre-curing time is prolonged from 3 to 5 min, and shows a sharp decrease (12.97 kPa) with the pre-curing time of 7 min (Fig. 2e). It is speculated that the compositions of the upper and bottom layers might interfere with each other under too short a pre-curing time (3 min). On the contrary, excessive pre-curing (7 min) is disadvantageous for efficient interfacial bonding since the inter-diffusion and chelation around the interface are largely weakened. Consequently, a pre-curing time of 5 min generates the best mechanical performance of the double-layer hydrogel, which is optimized for the following experiments.
The chelation between sodium alginate and calcium ions is beneficial for the interfacial bonding between the two layers. As shown in Fig. 3, the double-layer hydrogel without chelation could resist the shear deformation of only 16.1%, much lower than that of the chelated double-layer hydrogel (70.5%, Fig. 2b). The distinct discrepancy between pure upper- or bottom-layer hydrogels (critical deformation higher than 50%) reveals that the disruption originates from the interface. Meanwhile, the modulus of the double-layer hydrogel (13.68 kPa; Fig. S2 (ESI†) and Fig. 3d and e) is lower in comparison with that of the hydrogel with chelation (14.97 kPa, Fig. 2e). In addition, the interfacial bonding is still maintained to a certain extent after mineralization, considering that the mineralized double-layer hydrogel has a critical deformation strain of 56.1% (Fig. 3d) and a G′ value of 19.21 kPa (Fig. 3e and f).
The as-prepared bilayer hydrogel shows an opaque white appearance in the upper layer and a transparent appearance in the bottom layer. This non-uniform hydrogel becomes wholly opaque after lyophilization (Fig. S3a, ESI†). The swelling ratio of the hydrogels was examined by immersion in deionized water (Fig. S3b, ESI†). The bottom layer exhibits a higher swelling ratio (approximately 650%) than that of the upper layer (approximately 470%), and the swelling ratio of the bilayer hydrogel lies in between (about 540%). The excellent swelling behavior of the hydrogels is probably due to the hydrophilic groups such as amine, amide, hydroxyl and phosphate in each layer. The affinity of AAm, VPA and alginate for water is regarded as being higher than those of GelMA and AGA,38,39 which generates a higher swelling ratio for the bottom layer. To clarify this heterogenous property of the bilayer hydrogel, SEM was adopted to characterize the interior structure of the hydrogel. As shown in Fig. 4a, a clear boundary between the upper and bottom layers can clearly be recognized from the SEM image. The upper layer possesses large pores with an average size of 217 μm (Fig. 4d), while the bottom layer exhibits interconnected smaller pores (82 μm on average) (Fig. 4e). After mineralization, a significant swelling behavior can be visualized in the bottom layer as the size of the pores increases to about 112 μm (Fig. 4f). The statistical pore size of each layer is summarized in Fig. 4g, h and i, which confirms the heterogenous architecture of the bilayer hydrogel. Generally, large interconnected porosity is advantageous for cell infiltration, mass transport and vascularization.40 A macroporous hydrogel (a pore size above 10 μm) with a high pore size is thus usually sought.41 As reported in previous studies, larger pore sizes could drastically improve chondrogenesis, whereas the sub-chondral phase favours smaller pore sizes.4 Although a consensus has not been reached for the specific pore size for chondrogenic or osteogenic differentiation in various studies,42–44 the pore size of 100 μm is reported to be beneficial for vascularisation and bone ingrowth.45 In this regard, it is anticipated that the pore size of the hydrogel in our experiments could meet the requirements for bio-functionality. In addition, the pore size of the hydrogel is closely associated with the mechanical properties of the hydrogel, where, usually, the stiffness of the scaffold decreases as the porosity increases.46 For a higher stiffness of the bone layer in our experiments, smaller pore size is sought. It should be mentioned that the pores are interconnected with each other, as shown by the reconstructed micro-CT images of the double layer hydrogel (Fig. S4, ESI†) and SEM images of the hydrogel at different sites (Fig. S5, ESI†). To summarize, the mineralized bilayer hydrogel maintains a pore size of 100–300 μm, which is suitable for cell infiltration and vascularization.
For the hydrogel after mineralization, a thin layer of minerals was deposited on the surface of the polymeric network, even on that of the inner hydrogel (Fig. 4b), suggesting an in-depth mineralization process. Compared with the broad peak of an amorphous hydrogel without mineralization, the XRD pattern of a mineralized hydrogel shows intense sharp peaks, further confirming the existence of crystalline minerals (Fig. 4c). The diffraction peaks at 2θ = 31.6° and 2θ = 33.4° correspond to the (211) and (300) planes of hydroxyapatite (HAP). The strong diffraction peak at 2θ = 44.5° is possibly attributed to the (203) plane. Besides, other crystalline forms of calcium phosphate, such as dicalcium phosphate dihydrate (DCPD) and octacalcium phosphate (OCP), are also detected.
In order to reveal the effect of minerals on the mechanical properties of the hydrogel, the compressive stress–strain curves for hydrogels of different groups were measured (Fig. 4j), and the compressive modulus values calculated from the curves are listed in Fig. 4k. The upper layer exhibits a relatively soft and brittle property with a modulus of 81 ± 25 kPa and a stain of less than 55%. In comparison, the bottom layer possesses an enhanced modulus (112 ± 7 kPa) and a larger strain (68%), while the bilayer hydrogel shows an intermediate modulus (111 ± 12 kPa). After mineralization, the modulus of the bottom layer further improves to 132 ± 7 kPa with a decrease in the strain (58%), suggesting that the mineralization strengthens the modulus and stiffness of the hydrogel. Interestingly, for the mineralized bilayer hydrogel, its modulus decreases slightly to 106 ± 4 kPa, which might be explained by the weakening of the chelation between calcium ions in the upper layer and alginate in the bottom layer caused by mineralization (as confirmed by the rheological properties of the hydrogel before and after mineralization in Fig. 2 and 3). The mechanical properties of the hydrogel alter from the upper to the bottom layer, and satisfy the needs for chondrogenic and osteogenic differentiation of stem cells, respectively.16,35 Overall, the mineralized bilayer hydrogel has a suitable pore size, mechanical properties and, more importantly, a matched chemical composition with the ECM of natural osteochondral cells, so its biochemical properties are explored in the following.
Osteogenic differentiation is a cell-mediated process, during which some osteogenic-related genes are activated, and the secreted proteins are promoted. Here, the osteogenic differentiation of BMSCs was assessed on the bottom-layer hydrogel. The key osteogenic markers, Col-I and ALP activities, were detected after cultivation for 7, 14 and 21 days.47 The secretion of Col-I and ALP activities increased continuously with the passage of time (Fig. 5g and h). Compared with the pAAm and pAAm-VPA groups, the production of Col-I and ALP by the pAAm-VPA@M group is significantly enhanced. In particular, after 14 days of incubation, compared with pure pAAm (171 U per g protein) and pAAm-VPA (224 U per g protein), the pAAm-VPA@M group (838 U per g protein) exhibits ALP activity that is 3.7-fold higher. As the incubation time was extended to 21 days, the ALP secretion in all three groups increased and the superiority of the pAAm-VPA@M group was maintained.
Thereafter, the expression of osteogenic differentiation-related genes, Runx2, Col-I and OCN was monitored using the pure culture plate as a reference. As shown in Fig. 5i–k, generally, pAAm-VPA@M apparently elevated Runx2, Col-I and OCN gene expression over 21 days of culture in comparison with pAAm and pAAm-VPA. In detail, the expression of Runx2 was the highest on day 7 and then declined afterwards. By contrast, Col-I and OCN displayed growing expressions from 7 to 21 days. The expression of these genes accords well with the rhythm of osteogenic differentiation.48 As for the pAAm and pAAm-VPA groups, the introduction of VPA had an adverse effect on osteogenic differentiation, given that the expressions of Runx2, Col-I and OCN were attenuated to some extent. All these results confirm that pAAm-VPA@M is suitable as a scaffold for the repair of sub-cartilage bone, in consideration of its excellent osteogenic differentiation ability.
Next, to investigate the effect of the hydrogel on chondrogenic differentiation, the cell activity of the chondrocytes was evaluated by measuring the protein synthesis on the upper-layer hydrogel. As the main components of the cartilage extracellular matrix (ECM),50 the Col-II and GAGs levels were detected via ELISA kit at set time intervals (Fig. 6g and h). The contents of Col-II for all three groups showed not much difference on Day 7, and ascended slowly during further incubation. Chondrocytes on the GelMA–AGA surface produced remarkably higher levels of Col-II than the other two groups on Day 14 and Day 21. In addition, the secretion of another essential chondrogenic component, GAGs, is closely related to AGA. No significant differences are observed for the concentration of GAGs on PEGDA and GelMA, while GAGs on GelMA–AGA showed an apparent increase in comparison. The secretion of Col-II and GAGs together confirms that AGA in the hydrogel facilitates the chondrogenic activity.
Meanwhile, the gene expressions of chondrogenic markers, Col-II, SOX9 and AGG, were assessed to predict the trend of chondrogenesis by the hydrogels (Fig. 6i–k).51 The gene expressions of Col-II and SOX9 for the GelMA–AGA group were the highest among the three groups on Day 7 and Day 21. Similarly, the AGG expression on GelMA–AGA was superior to that on PEGDA and GelMA over the whole incubation, and was significantly higher on Day 21 (Fig. 6k). By contrast, the expressions of chondrogenic markers for the PEGDA and GelMA groups were lower and approximately equal with each other. Based on the above results, AGA is beneficial for chondrogenic differentiation, while the effect of GelMA is not comparable. Therefore in the following experiments, GelMA–AGA was chosen for fabrication of the upper-layer scaffold.
The appearance of the hydrogels was observed after 1, 4 and 8 weeks of implantation. The yellow dotted circles in Fig. 7a–c illustrate the outlines of the hydrogels. The areas of the hydrogels exhibited a tendency for reduction and the weight of the hydrogels also decreased (Fig. S8, ESI†), which is ascribed to their slow degradation in vivo. Even so, it might take more time for complete degradation, considering the fact that the hydrogels still exist after 8 weeks. To evaluate the inflammation, the subcutaneous tissue around the hydrogel was observed. As illustrated in the inset of Fig. 7a, the tissue wrapping the hydrogels was red and inflamed from the examination after one week, which can also be seen from the surrounding tissue fluid in the side view. However, the inflammation response subsided after 4 weeks (Fig. 7b). Furthermore, near-normal subcutaneous tissue with no inflammation was observed after 8 weeks (Fig. 7c), and the hydrogel was well integrated with the surrounding tissues (inset in Fig. 7c).
H&E staining was then applied to further analyse the inflammation of the subcutaneous tissues. As shown in Fig. 7d and g, a massive accumulation of macrophages (indicated by the black arrows in Fig. 7d and g) in both groups represents the acute inflammatory reaction during the early period (one week). This situation changed after 4 weeks of implantation. Significantly reduced inflammatory cells were observed, although some still remained in the subcutaneous fascia and muscles (Fig. 7e and h). After 8 weeks, an attenuated inflammatory response was detected, given that only sporadic inflammatory cells could be found (Fig. 7f and i). The inflammation of the hydrogel group does not show any significant differences with the control groups during the whole period. Tissue inflammation was also blindly scored for better illustration.26 As shown in Fig. S9 (ESI†), the scores of both groups were about 3 after one week, which meant obvious inflammation. After 4 weeks, the scores declined to about 2, suggesting inflammation relief in small areas. After 8 weeks, the scores further reduced to about 1, showing signs of mild inflammation. There is no significant difference between the control and the hydrogel groups. The decline of the inflammatory response for the hydrogel group might be originating from the degradation of the hydrogel, considering that a sustained inflammatory response could occur for the implantation of non-degradable materials.52
In addition, the inflammatory response markers TNF-α, IL-1β and IL-6 were quantitatively measured to evaluate the tissue inflammation.53,54 TNF-α is an important cellular inflammatory factor, which is mainly produced by monocytes. As shown in Fig. 7j, both groups produced considerable TNF-α (about 51 pg mL−1) after 1 week of implantation, suggesting that acute inflammation occurred. The concentration of TNF-α in the hydrogel group was slightly higher than that of the control group. After 4 and 8 weeks, the secretion of TNF-α in both groups constantly decreased, while the TNF-α level of the hydrogel group gradually fell below that of the control group. No significant differences are observed for both groups during the whole of the 8 weeks. This phenomenon indicates the good biocompatibility of the hydrogel.
Interleukins (ILs) are an essential category of cytokines, among which IL-1β and IL-6 play a significant role in the immune regulation and inflammatory response processes.55,56 The pattern of IL-1β secretion is illustrated in Fig. 7k. Similar to the tendency of TNF-α, both the groups exhibited high levels of IL-1β in the early stage. The amount of IL-1β drastically decreased after 4 weeks, and remained almost the same after 8 weeks without any significant difference between the two groups. This result confirms the existence of acute inflammation during the early period. After that, the inflammation response gradually subsided and finally reached a plateau. Another cytokine, IL-6, secreted by T cells and macrophages, stimulates the immune response and resists infection.57,58 Both groups showed no obvious changes in IL-6 during the whole process (Fig. 7l), which indicates the sustained anti-inflammation response. In brief, there were no significant differences between the control and experimental groups with respect to the three markers, proving the acceptable compatibility of the bilayer hydrogel with subcutaneous tissues.
Micro-CT is utilized to analyse the content of bone minerals in our experiments. As illustrated in Fig. S10a (ESI†), the tissue surrounding the hydrogel in all 4 groups was initially regenerated to different extents, especially the superficial area. The superficial defects of the bilayer group exhibited better regeneration compared with those of the other groups. A volume of interest (VOI) was established for each group for comparison (Fig. S10b, ESI†). The ratio of the bone volume fraction to the total volume (BV/TV), and the bone mineral density (BMD) of the bone volume fraction and of the total volume were calculated from micro-CT results. As shown in Fig. S10c–e (ESI†), all three parameters measured in the bilayer groups were higher than those in the other groups, although the advantage was not significant.
To thoroughly evaluate the repair ability of the different hydrogels, the collected osteochondral samples were sectioned and stained for histological analysis. As shown in Fig. 8d, the typical layered structure of cartilage to bone was not observed in the control group, although an irregular arrangement of cells in the superficial area and a loose fibrous structure in the middle of the defect were visualized. By contrast, newly formed tissues displayed the characteristic layered structure in the three hydrogel groups. In the upper-layer group, the regenerated cartilage tissues exhibited a fibrocartilage-like appearance, as evidenced by an intense Masson staining of Col-I in the upper region (Fig. 8d and Fig. S11, ESI†).60 In both the bottom-layer and bilayer groups, the arrangement of cells exhibited a slight trend of being parallel with the surface in the superficial area, whilst being vertical to the surface in the deeper zone, similar to that of natural articular cartilage. The expression of Col-I and Col-II was mainly located in the subchondral and articular areas, respectively (Fig. S11 and S12, ESI†). This phenomenon is similar to the distribution in natural tissue.61 It is noteworthy that the bilayer group induced a thicker regeneration of articular tissue. Apart from that, the formation of new bone in the subchondral zone was distinctly detected for the bottom-layer hydrogel. All these results confirm that the bilayer hydrogel regenerates more intact structures of the defect area, and is advantageous for osteochondral tissue engineering.
We have to admit that although preliminary regeneration has been achieved, this work still has some limitations. Rabbits have a high regenerative ability and different skeletal structures from those of human beings. Hence, large trials should be devoted to confirming the regeneration ability in a real human body environment. Besides, the mechanical properties of the bottom-layer hydrogel could also be improved by the introduction of another network or more inorganic components. Furthermore, the immunomodulatory effects for osteochondral repair will be considered in our further studies.62,63
Footnotes |
† Electronic supplementary information (ESI) available: Hydrogel formulas for in vitro cell study, the sequences of primers used for real-time PCR, frequency sweeps for hydrogels of different groups, photographs and swelling ratios of hydrogels, SEM images of double-layer hydrogels of different sites, fluorescence microscopy images of chondrocytes cultured on upper layers of hydrogels for 7 days, body weights of SD rats in different groups post-surgery, scores of H&E stains in subcutaneous tissue, 3D reconstruction of samples of different groups, the reconstructed VOI images of defect areas for different groups, bone volume/total volume (BV/TV), bone mineral density of total volume (BMD of TV), and bone mineral density of bone volume (BMD of BV) calculated from micro-CT results, and collagen-I and collagen-II stains of collected knee joints after 6 weeks of implantation. See DOI: 10.1039/d1tb00518a |
‡ Zhuoxin Chen and Hong Xiao contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2021 |