Kai D.
Knight
a and
Megan E.
Fieser
*ab
aDepartment of Chemistry, University of Southern California, Los Angeles, CA 90089, USA. E-mail: fieser@usc.edu
bWrigley Institute for Environment and Sustainability, University of Southern California, Los Angeles, CA 90089, USA
First published on 27th November 2023
A pyridine diimine cobalt catalyst series is used for the cyclodepolymerization (CDP) of several different polyesters and polycarbonates. In the presence of isopropanol, a wide range of polymers can undergo solvolytic depolymerization. CDP of poly(propylene carbonate) revealed an unzip back-biting or random scission mechanism, depending on what conditions were used. The first example of a method capable of solvolysis and CDP on a polymer mixture in the same pot is identified.
Many polyesters and polycarbonates can be made from bio-feedstocks.3 Polyesters are often considered degradable or compostable. However, these strategies often need industrial composting, which requires an additional collection stream.3,4 While these composting methods allow for polymer degradation to CO2 to occur, the value of the chemical is not retained quickly, as a chemical that can be readily converted back to polymer is not produced. This requires vast biofeedstock sources to be grown annually.5,6 Alternatively, even if considered biodegradable, polycarbonates are often resistant to degradation, highlighting the need for different strategies to manage their end of life.7,8
These materials can also be chemically recycled, adding another strategy to recover valuable chemicals that can be used to remake the polymer directly.3,9–11 For polyesters and polycarbonates, there are four primary methods for chemical recycling: hydrogenation, transfer hydrogenation, solvolysis and cyclodepolymerization (Fig. 1 and 2).3,9,12 Each of these methods have their advantages and challenges, and some methods are better for specific polymers.
Fig. 2 Possible cyclodepolymerization pathways for polycarbonates (a) to trans-carbonate (i), cis-carbonate (ii), and epoxide and carbon dioxide (iii) and for polyesters (b). |
Hydrogenation often breaks polyesters and polycarbonates down into diols, which are useful for numerous applications, including synthesizing new polymers.12–14 However, high pressures and temperatures are often used, posing safety and energy challenges. A safer alternative, albeit less atom economical, is transfer hydrogenation, which uses a hydrogen source like isopropanol to generate an equivalent of H2 and acetone as a by-product. Though apart from numerous examples of the transfer hydrogenation of lignin, few reports exist documenting the transfer hydrogenation of polymers.15–17
Solvolysis remains one of the most studied methods for the depolymerization of step-growth polyesters, particularly for poly(ethylene terephthalate) (PET).11,18 The use of water, methanol or ethylene glycol can lead to linear molecules that can be used again for polymerization.19,20 Hydrolysis is relevant to many polyesters and polycarbonates, however these materials are often insoluble in water and need harsh conditions to reach efficient depolymerization.21 Methanolysis and glycolysis may be more useful depolymerization methods, as is the case with PET, in which the product may regenerate new PET.22–24 Finally, the cyclodepolymerization (CDP) of polyesters and polycarbonates back to their cyclic precursors is an emerging area of research, as this method often applies to chain growth polymers, which are receiving much interest as replacements for non-degradable polymers. In many cases, the ceiling temperature of the polymer makes a big difference on how cyclodepolymerization can occur.25–35 Additionally, high dilution of the reaction often allows for higher conversion to cyclic monomer, albeit with the crucial flaw of requiring large amounts of solvent.36,37 Recently, reports of manipulating ceiling temperature combined with reactive distillation methods have prevented the need for high dilution.38–40 Namely, Byers and co-workers reported exciting catalysts for the CDP of many polyesters and polycarbonates at high yields using a reactive distillation method.40
CDP of polycarbonates can take two forms: either formation of cyclic carbonates or complete depolymerization to epoxides and CO2 (Fig. 2a).9 There are few examples of CDP of commercial polycarbonates and polyesters to their respective cyclic monomers.41–44 In this case, CDP of the polycarbonate often leads to a cis-cyclic carbonate, a product which lacks examples of being polymerized. Many of these examples have shown the ability to perform CDP on specially designed polymers, which have been modified or synthesized with the intention that these polymers also cyclodepolymerize to polymerizable monomers.26,28,29,31,33,34,38,45–49 Similarly, scant examples of complete CDP to epoxides and CO2 exist in the literature.50–53 To date, there is still not a clear understanding for what catalysts lead to selectivity of either form of CDP, although computational studies have helped rationalize a catalyst's ability to lower the barriers for a specific method.49 CDP of polyesters has one main pathway to generate cyclic esters (Fig. 2b). Examples of CDP for common polyesters, such as poly(ε-caprolactone) (PCL), poly(δ-valerolactone) (PVL), polydioxanone (PDO), poly(caprolactam) (nylon-6), and poly(lactic acid) (PLA) are known with metal catalysts.35,40,44,45,54
Herein, we demonstrate the use of a pyridine diimine cobalt catalyst that can catalyse the cyclodepolymerization of several different polyesters and polycarbonates. In the presence of isopropanol, these catalytic methods also facilitate solvolytic depolymerization of seven different polyesters and polycarbonates, which is attributed to the base used in the reaction. To our knowledge, this is the first example of a single catalyst system demonstrating these two depolymerization strategies. We demonstrate proof of concept for achieving both methods in the same pot, which addresses considerations of mixed polymer waste.
Using transfer hydrogenation conditions of poly(propylene carbonate) (PPC), inspired by the recent work from Werner and coworkers, these cobalt complexes did not show any evidence for the formation of the expected transfer hydrogenation products: propane diol and methanol.15 Instead, exclusive formation of propylene carbonate (PC) was observed for all three catalysts, with reactions yielding PC, cyclodepolymerized from PPC, within 20 h at 140 °C (Table 1, entries 1–3).
Entry | Catalyst | Time (h) | KOtBu (mol%) | Solvent(s) used | Solvent volume (mL) | % Yieldb,c |
---|---|---|---|---|---|---|
a Conditions: 5 mol% catalyst with respect to the repeat unit molar mass of the polymer, 2 mmol PPC, run at 140 °C and 350 rpm in Parr reactor. Reactions with KOtBu were performed in an air-free, N2 environment. All other entries were performed exposed to air. b Determined by comparing 1H NMR spectroscopy using mesitylene as internal standard, taken in CDCl3. c Parentheses next to yields indicate reactions performed in duplicate; standard deviation of error in parentheses. d NMR calculation used in place of internal standard yield calculation due to neat method's challenges in collecting full product. | ||||||
1 | MES | 20 | 5 | iPrOH:THF | 8:2 | 66 |
2 | DIPP | 20 | 5 | iPrOH:THF | 8:2 | 66 |
3 | DEP | 20 | 5 | iPrOH:THF | 8:2 | 64 |
4 | MES | 20 | 5 | THF | 6 | >99(0) |
5 | DIPP | 20 | 5 | THF | 6 | 78(19) |
6 | DEP | 20 | 5 | THF | 6 | 97(3) |
7 | MES | 20 | 0 | THF | 6 | 81(3) |
8 | DIPP | 20 | 0 | THF | 6 | 55(45) |
9 | DEP | 20 | 0 | THF | 6 | 99(2) |
10 | DEP | 10 | 5 | THF | 6 | 83(3) |
11 | DEP | 10 | 0 | THF | 6 | 69(4) |
12 | DEP | 10 | 10 | THF | 6 | 89(3) |
13 | DEP | 6 | 5 | THF | 6 | 87 |
14 | DEP | 6 | 10 | THF | 6 | 99 |
15 | DEP | 10 | 0 | 2-Methyl THF | 6 | 15 |
16 | DEP | 10 | 0 | PhCl | 6 | 25 |
17 | DEP | 10 | 0 | Toluene | 6 | 12 |
18 | DEP | 10 | 0 | THF:PC | 3:3 | 86(2) |
19 | DEP | 10 | 0 | PC | 6 | 93(1) |
20d | DEP | 10 | 0 | None | 0 | >99(0) |
21 | DEP | 6 | 0 | THF | 6 | 52(9) |
22d | DEP | 6 | 0 | None | 0 | 89(1) |
23 | None | 10 | 5 | THF | 6 | 41 |
Notably, the PPC reaches a temperature threshold of 170 °C, at which point, the polymer is known to degrade/depolymerize into PC.61,62 For this polymer, this temperature allows for the conversion of the kinetic polymer product (PPC) to the thermodynamic cyclic carbonate (PC).7,8,42
Once CDP selectivity was identified for these cobalt catalysts, efforts to optimize the reaction conditions for this method over transfer hydrogenation was prioritized. A tetrahydrofuran (THF)/isopropanol (iPrOH) mixture with potassium tert-butoxide (KOtBu) was used to replicate Werner's transfer hydrogenation conditions.15 THF was used to solubilize the polymer, isopropanol as the hydrogen source, and KOtBu as a strong base.15 These conditions may not be necessary to produce PC. Without iPrOH, MES and DEP catalysts reached quantitative conversion within 20 hours at 140 °C, with DIPP displaying high but inconsistent yields of PC (Table 1, entries 4–6). These results indicate that the hydrogen source is unnecessary. CDP reactions conducted without this base yielded very similar results, if not slightly lower conversions, to those with base, save for that of DIPP, indicating base was not significantly impacting the rate of CDP (Table 1, entries 7–9).
When comparing the ligand substituents, the catalyst with mesityl (MES) and diisopropyl phenyl (DIPP) substituents showed slower CDP of PPC, while the catalyst with ethyl substituents (DEP) proved fastest and the most reproducible amongst the three ligands. DIPP is hypothesized to have too much steric crowding to allow for facile backbiting on the polymer. It is unclear why MES is slower than DEP, however solubility could be a challenge, as these catalysts are only mildly soluble in THF at room temperature. Given DEP's speed over DIPP and MES in the optimized conditions without iPrOH or base, this catalyst was used for further optimization. With DEP (Fig. 3), reactions shortened to 10 hours in THF showed a distinct difference when KOtBu was used (achieving 83% yield) versus when KOtBu was not used (achieving just 69% yield) (Table 1, entries 10 and 11). These results indicate that presence of base does increase the rate of CDP when considering reactions that have not reached high conversions. It is anticipated that the initiation of the reaction occurs through the deprotonation of the polymer end group, which is likely an alcohol, or through nucleophilic attack of a carbonyl on the polymer chain (Fig. 4a). An OtBu alkoxide would likely be faster than a chloride for both proposed routes, supporting the higher yield of PC with KOtBu present.
Fig. 4 Proposed mechanisms for initiation (a), catalysis and subsequent side reactions (b) of CDP of PPC. |
One hypothesis is that the base could exchange the Cl ligands with the –OtBu ligands, which might enhance nucleophilic attack of carbonyls in the polymer and increase the initiation rate of depolymerization. This reaction has been conducted on similar Fe complexes with PDI ligands.63 Notably, reactions with KOtBu show a rapid color change from yellow brown to purple when solvent is added to the reaction mixture. This color change is not observed without the presence of KOtBu. In this case, two equivalents of KOtBu would be needed to exchange with all the chlorides on DEP. This indeed shows slightly faster conversion than DEP with one equivalent of KOtBu (Table 1, entry 12). Additionally, stirring DEP with one or two equivalents of KOtBu prior to the addition of PPC lead to even higher conversions, indicating the likelihood that exchanging the Cl anions for OtBu anions increases the reactivity of the DEP catalyst (Table 1, entries 13 and 14). Unfortunately, the low solubility of DEP in most solvents at room temperature prevents the ability to characterize this exchange either by NMR spectroscopy or isolation in bulk. Future directions aim to adjust the ligands for increased solubility to confirm these hypotheses.
Once the metal catalyst has the polymer chain bound, the expected mechanism of CDP with metal-based catalysts is back-biting from alkoxide or carbonate end groups bound to the metal ion. These end groups could perform consistent back-biting reactions to directly form PC, depolymerizing the polymer through a controlled “un-zip” pathway (Fig. 4b). Additionally, the end groups could perform transesterification reactions further down the polymer chain to form cyclic oligomers or on another polymer chain which changes the polymer molar mass (Fig. 4b). Indeed, these proposed mechanisms are well-documented across several PPC depolymerization studies.9,40,42,64 From these suspected routes, it was important to understand if reaction conditions could impact rate of CDP and control for the desired “un-zip” pathway.
Since KOtBu is moisture-sensitive, reactivity of the catalyst without base was investigated, with the reactions pursued in the presence of air. DEP is air stable and can be left over a month without showing decomposition. Using the standard reaction conditions taken from Table 1, entry 11, batch reactions were performed to follow the progress of the reaction (Fig. 5). Yields were characterized by 1H NMR spectroscopy. The remaining PPC was also characterized by size-exclusion chromatography (SEC). Within the first 4 hours, only slow CDP is observed, while the rate rapidly increases, demonstrating a more linear trend, over the next 8 hours to reach a total conversion of 94% after a total of 12 hours. The slow initial rate of CDP suggests an induction period, which could be due to the low basicity of the chloride anions to deprotonate chain ends of the PPC. Once all catalysts are bound to polymer chains, this could explain the increase in rate. Before all polymer chains are deprotonated, chain transfer could occur and slow productive CDP. Following the reaction by SEC showed a consistent decrease in the dispersity of the remaining polymer chains. A duplicate reaction series shows the same general trend (see ESI†). Random nucleophilic attack on the polymer would likely result in broad and/or multimodal molar mass distributions, as there would be no preference for reacting with any particular part of the polymer chain. Monomodal molar mass distributions, along with the decrease in dispersity, suggest that these side reactions are not occurring, indicating selective “un-zip” backbiting reaction for CDP of PPC with PDICoCl2 catalysts.
Fig. 5 SEC traces for CDP of PPC with DEP in THF at 140 °C for different time points, using light scattering (LS). Note, the red trace labelled PPC is the SEC trace of the PPC starting polymer. |
It was anticipated that the presence of base could lower the induction period, which would lead to productive CDP faster than without base. Other air-stable bases in addition to KOtBu were tested (Table 2). Two of the bases, NaOH and NaHCO3, presented diminished yields in comparison to analogous conditions without base. NEt3 showed a similar yield to that without base. Two bases (KOH and NaOtBu) resulted in comparable yields to that with KOtBu, without the need for inert conditions. These results indicate that a stronger base or easier ability to exchange the chlorides on DEP may be important to improve the reaction rate. Running time points with NaOtBu, analogous to those done without base in Fig. 5, showed inconsistent yields. Notably, reactions that did not reach full conversion with NaOtBu displayed a higher dispersity than the original PPC starting polymer (ESI Table S4†). Returning to KOtBu time points showed a more consistent increase in conversion over time. However, with this base, dispersity was variable, suggesting random chain scission. Interestingly, this similar pattern of variable dispersity with CDP is seen with use of ZnEt2 from Byers et al.40 These results suggest that the base could be performing side reactions with or without the use of the catalyst, leading to random scission and less controlled CDP. Control reactions with KOtBu alone did show mild conversions of PPC to PC, indicating they can facilitate CDP with and without the catalyst (Table 1, entry 23). These conditions contrast those seen with the unzipping mechanism without base. Though the chloride from DEP alone proved better at unzipping, this may be in part due to halides being weaker nucleophiles than alkoxides, making them more likely to attack end groups because of their proximity.
Entry | Base | Time (h) | % Yieldb,c |
---|---|---|---|
a Conditions: 5 mol% DEP and 5 mol% base with respect to the repeat unit molar mass of polymer, 2 mmol PPC, 6 mL THF, 350 rpm, run at 140 °C in Parr reactor. Reactions performed under air-free N2 atmosphere if KOtBu used, otherwise performed in air. b Determined by 1H NMR spectroscopy using mesitylene as internal standard, taken in CDCl3. c Reactions performed in duplicate; standard deviation of error represented in parentheses. | |||
1 | KOH | 10 | 79(8) |
2 | NaOH | 10 | 58 |
3 | NaHCO3 | 10 | 24 |
4 | NEt3 | 10 | 61 |
5 | NaOtBu | 10 | 86(1) |
6 | KOtBu | 10 | 83(3) |
7 | NaOtBu | 2 | 40(14) |
8 | NaOtBu | 4 | 58(15) |
9 | NaOtBu | 6 | 50(12) |
10 | NaOtBu | 8 | 44(12) |
11 | NaOtBu | 12 | 65(16) |
12 | KOtBu | 2 | 74(0) |
13 | KOtBu | 4 | 85(3) |
14 | KOtBu | 6 | 91(2) |
15 | KOtBu | 8 | 92(2) |
16 | KOtBu | 12 | 92(2) |
While THF was originally used, analogous to prior transfer hydrogenation reactions, the solvent scope was further tested to promote the fastest catalysis. Reactions performed in chlorobenzene, 2-methyl THF, and toluene did not facilitate rapid CDP, showing diminished yields to those conducted in THF (Table 1, entries 15–17). The use of PC or a PC/THF mixture both led to higher yields than those with just THF. This could be due to the higher boiling point of PC, which maintains solubility of the polymer and catalyst at elevated temperatures (Table 1, entries 18 and 19). These results suggested that the reaction could be done with polymer in the melt without added solvent, where the generated PC becomes the solvent over the course of the reaction. Gratifyingly, full conversion of PPC to PC was achieved within 10 hours when the reaction was conducted on PPC in the melt without solvent addition, in which no remaining PPC is observed by NMR spectroscopy (Table 1, entry 20). An 89% yield is achieved in just 6 hours with these neat conditions, compared to 52% yield with THF (Table 1, entries 21 and 22). This is the first example for CDP of PPC in the melt without a solvent. To ensure that presence of PC in the reaction does not lead to polymerizations, control reactions were conducted with DEP or KOtBu with PC as monomer and THF as solvent for 10 h at 140 °C, with no PPC formation observed (see ESI†). While reactions done with PPC in the melt could lead to greener methods for CDP, quantification of the products was more difficult if the reaction did not reach full conversion, therefore further studies were still conducted in the presence of solvent.
To identify how reaction concentration impacts CDP of PPC with DEP, the reaction concentrations were varied in two ways. In one method, the PPC and catalyst quantities were kept constant, while the THF volume was varied (Fig. 6a, blue). While this method showed no observable pressure differences on the Parr reactors as the volume of THF increased (maintaining a steady 6.0 bar), it was important to rule out any pressure contributions to the data. Therefore, the second method kept the THF volume constant, while the PPC and catalyst quantities were varied (Fig. 6a, orange). Both methods showed the same overall outcome, suggesting that pressure is not impacting the results. Four different concentrations were measured, with the most concentrated and second most dilute conditions showing the highest yields for CDP. The higher concentration reactions could show higher yields due to the catalyst initiating CDP faster, while also increasing the rate of the metal ion coming in proximity to the next carbonyl on the polymer chain. This condition also most closely matches conditions in the melt, which has shown the highest yield. The metal center could be performing chain transfer reactions between polymer chains. Dilution could prevent this side reaction. However, over-dilution could slow the metal from initiating CDP.
Next, varying the catalyst loading, while maintaining all other conditions, showed an expected increase in yield as the catalyst loading is increased from 0.5 to 5 mol% (Fig. 6b). However, when catalyst loading is increased to 7.5 mol%, a drop in yield is observed. It is unclear what causes this drop in yield, though, the added concentration of metal bound to polymer chain could lead to increased presence of chain transfer or the presence of transesterification of other polymer chains, leading to lowered back-biting (Fig. 7). With smaller amounts of catalyst in fewer quantities than the polymers’ available end groups, the cobalt-alkoxide (or carbonate) may either backbite for productive PC formation or deprotonate for chain transfer, reducing efficiency of the reaction (Fig. 7a). Yet when catalyst outweighs the number of available polymer end groups, transmetalation may compete with CDP as a reaction (Fig. 7b). Based on the molar mass (Mn) of the PPC starting material, there is an approximate 10:1 ratio between DEP and polymer end groups. This would indicate that these conditions lie in the Fig. 7b region or it could suggest there is just a point at which too much DEP inhibits productive CDP. Control reactions with catalyst concentrations that are low (2.5 mol%) and high (7.5 mol%) were conducted for 2 and 6 hours, in which the remaining polymer was characterized by SEC (see ESI†). In both cases, dispersity still remained low at 2 hours, while 6-hour reactions showed an increase in dispersity. These results support the hypothesis that catalyst loading needs to match the end group concentration for the CDP to remain controlled.
Fig. 7 Proposed side reactions to understand catalyst loading effects when comparing lowered catalyst loading (a) to increased catalyst loading (b). |
The ideal temperature range for the reaction was then probed with DEP, as increased temperatures have the potential to increase CDP (but may also provoke side reactions), by nearing PPC's degradation temperature of 170 °C.61 Fortunately, high selectivity and higher conversions were maintained with increased temperature, as the reaction reached near full conversion in 10 hours at 140 °C and quantitative conversion at 160 °C (Fig. 6c). This indicated that use of DEP fully depolymerized PPC within the range of 140–160 °C, but reaction optimization conditions were maintained at 140 °C to better distinguish which conditions were more efficient. Compared to the first reported degradation of PPC to PC by Kuran et al., use of DEP requires less solvent and catalyst while producing higher yields in a shorter amount of time.43 When compared with more recent studies, like that of Kerton et al. or Darensbourg et al., the use of DEP under these conditions offers somewhat of a trade-off in certain areas.41,42 While use of DEP requires a metal catalyst, slightly higher temperatures, and longer reaction times, the use of any solvent, much less those detrimental to the environment, can be forgone.
Fig. 9 Substrate scope of solvolysis with DEP and KOtBu. Catalyst and base loadings made with respect to the repeat unit molar mass of polymer. |
Since these two pathways seemed compatible with each other, we questioned whether they could be used in parallel in the same reaction mixture. PPC and PBPAC were selected to mix, as they are both polycarbonates, PPC shows exclusive CDP under all conditions studied, and PBPAC does not have an accessible cyclic monomer. Notably, in a mixed pot of PBPAC and PPC in a 1:1 molar ratio with respect to the repeat unit of the polymer, under conditions of DEP at 180 °C with KOtBu and isopropanol and THF as solvents, CDP was maintained with PPC while solvolysis prevailed with PBPAC to bisphenol A (BPA) and diisopropyl carbonate (DIPC) (Fig. 10), with both pathways reaching full conversion. Similarly, under conditions of just DEP with THF as solvent at 140 °C, PBPAC remained intact while PPC depolymerized to PC at 91% yield, which bodes well for isolating depolymerization products in mixed recycling streams. On the other hand, PVL under solvolysis conditions yield solvolysis products, indicating multiple depolymerization paths for one polymer with the same catalyst under different conditions.
Finally, extensions to other carbonyl-containing polymers identified these catalysts as highly active for the selective CDP of poly(δ-valerolactone) (PVL) and polydioxanone (PDO) with DEP alone. Activities of CDP for poly(trimethylene carbonate) (PTMC), poly(lactic acid) (PLA) and poly(ε-caprolactone) (PCL) were observed in smaller amounts, however optimization of the conditions or the catalyst may be needed to achieve high conversion. In the presence of KOtBu and iPrOH, DEP could promote solvolytic depolymerization of several commodity polymers. Control reactions identify the KOtBu shows comparable activity on its own, suggesting it is the active catalyst in this reaction.
The results of these studies were used in a proof of concept mixed-recycling stream of PPC and poly(bisphenol A carbonate) (PBPAC), in which solvolysis conditions lead to the full conversion of PPC CDP and PBPAC solvolysis. CDP conditions without base or iPrOH led to selective CDP of PPC to 91% conversion, with the PBPAC being left undisturbed. These results identify promising routes for tunable deconstruction of these polymers. Future work to identify optimal changes to the metal and ligands to further improve CDP of carbonyl-containing polymers are currently underway.
Footnote |
† Electronic supplementary information (ESI) available: X-Ray, NMR, FT-IR, and SEC data. CCDC 2292414. For ESI and crystallographic data in CIF or other electronic format see DOI: https://doi.org/10.1039/d3qi01833d |
This journal is © the Partner Organisations 2024 |