Jiayu
Zhang‡
a,
Yanfei
Li‡
b,
Yihan
Song
a,
Guoduo
Yang
a,
Zhuo
Wang
a,
Xinyao
Huang
a and
Haizhu
Sun
*a
aCollege of Chemistry, National & Local United Engineering Laboratory for Power Batteries, Northeast Normal University, No. 5268, Renmin Street, Changchun, 130024, P. R. China. E-mail: sunhz335@nenu.edu.cn
bState Key Laboratory of Organic Electronics and Information Displays & Institute of Advanced Materials (IAM), School of Chemistry and Life Sciences, Nanjing University of Posts & Telecommunications (NJUPT), Nanjing 210023, P. R. China
First published on 11th July 2025
The practical implementation of lithium metal remains challenging because of unregulated Li dendrite growth, which results in safety hazards and poor cycling performance. Herein, a stable three-dimensional (3D) hybrid architecture with low voltage hysteresis is fabricated by modifying N,O-codoped carbonized-polymer-dots (CPDs) on a carbon-based substrate (CPDs-GCC). CPDs provide an abundance of lithiophilic nitrogen-containing functional groups and carbonyl groups, which can direct the homogeneous deposition of lithium and reduce the growth of Li dendrites. Moreover, the CPD-based lithiophilic anode reduces the migration energy barrier and activation energy of Li+, enhances the exchange current density, and effectively enhances the ion transport kinetics and ion reaction kinetics at the electrode–electrolyte interface. As a result, the half cells with a capacity of 3 mAh cm−2 allow an ultralow voltage hysteresis of ∼2 mV over 4800 h at 2 mA cm−2. The full cell with a LiFePO4 cathode demonstrates outstanding cycling stability with a capacity retention of 95% after 3000 cycles at 0.2 A g−1. This study examines the factors influencing voltage hysteresis, explores its impact on battery performance, and proposes a simple method to mitigate it. This lays the foundation for the development of high-performance batteries.
Green foundation1. Compared to metal-based materials, carbon-based alternatives provide sustainable advantages through abundant sources and avoid mining/smelting processes, significantly reducing production energy and non-renewable resource dependence.2. This work demonstrates an ultra-low hysteresis Li anode via carbonized polymer dots (CPDs) on carbon current collectors. Different from metal-based systems, CPDs feature simple, green synthesis without organic solvents or toxic heavy metals (Ni, Co), preventing environmental contamination. 3. The use of biomass small molecules as precursors for the synthesis of CPDs can further diversify the raw material sources of carbon and enhance the potential for waste utilization. However, challenges remain in exploring the relationship between the structure of CPDs and the improvement of battery performance to select appropriate biomass small molecules. |
To address these issues, controlling Li nucleation behavior is important, which is known to be significantly impacted by matrix surface properties.19 Consequently, the modification of 3D current collectors has consistently been a key focus of investigation in this field. A successful modification will lead to a high coulombic efficiency (CE) and low voltage hysteresis. A high CE is typically indicative of enhanced anode utilization, while low voltage hysteresis is commonly correlated with improved cycling stability. For instance, Yang and co-workers produced a 3D current collector on copper foam that induced consistent and stable Li deposition by anchoring graphene, which maintained a CE of 97.4% at 2 mA cm−2 after 150 cycles and afforded an area capacity of 6 mAh cm−2 at 6 mA cm−2 in symmetric cells.13 Liu and co-workers reported a gradient-pore-size carbon skeleton as the lithium metal anode. The anode exhibited a modest and steady voltage polarization of ∼15 mV over 1000 h.20
Although substantial progress has been made in enhancing CE, research on voltage hysteresis remains limited. On the one hand, the concept of voltage hysteresis remains poorly defined, with many studies only superficially addressing it without elucidating the underlying mechanisms, which leads to voltage polarization being limited to approximately 10–20 mV in most materials. On the other hand, the relationship between voltage hysteresis and cycling stability is not well elucidated, hindering the analysis of abrupt changes in voltage hysteresis during long-term cycling. Therefore, investigating the factors influencing voltage hysteresis and their relationship with cycling stability is of great significance.
Herein, a novel strategy is developed to modify N,O-codoped carbonized polymer dots (CPDs) on the surface of cotton cloth covered with reduced graphene oxide (rGO), namely, CPDs-GCC, which can be applied as a 3D stable lithium anode substrate to achieve ultralow voltage hysteresis and enhance the cycling stability. The material surface is rich in functional groups, making it have tremendous potential to induce homogeneous nucleation and deposition of lithium metal.21–25 The electrode fabricated based on CPDs-GCC reduces the migration energy barrier and activation energy of Li+, increases the exchange current density, and effectively enhances the ion transport kinetics and ion reaction kinetics at the electrode–electrolyte interface. The experimental results show that the N,O-codoped CPDs significantly improve the lithiophilicity and enable stable operation for over 4800 h at 2 mA cm−2, with a voltage hysteresis as low as 2 mV in symmetric cells. Specifically, the full cell with a LiFePO4 cathode can maintain 95% capacity (139 mAh g−1) after 3000 cycles at 0.2 A g−1. Even under substantial deformation, the assembled flexible lithium metal batteries (FLMBs) retain outstanding flexibility and stability.
Carbonized polymer dots were prepared based on the classical hydrothermal synthesis method.26 The morphology of the synthesized CPDs is studied by transmission electron microscopy (TEM). Fig. S1a† shows the TEM images of CPDs with diameters in the range of 1.3–3.4 nm. The HRTEM image of CPDs in Fig. S1b† shows that the parallel plane spacing is 0.21 nm. A broad peak at 21° observed in X-ray diffraction (XRD) patterns indicates the low crystallinity of CPDs (Fig. S2†). As shown in Fig. S3,† the Fourier transform infrared (FT-IR) spectrum of the CPDs exhibits the stretching vibrations of –OH at 3430 cm−1, –NH at 2923 cm−1 and C–H at 2850 cm−1, the vibrational absorption band of CO at 1635 cm−1, the bending vibrations of N–H at 1570 cm−1, and the asymmetric bending vibrations of –C–NH–C– at 1126 cm−1. Through the survey X-ray photoelectron spectroscopy (XPS) spectrum shown in Fig. S4a,† abundant C, O, and N elements on the surface of the CPDs are confirmed to be present. According to the atom content listed in Table S1,† the contents of elements C, O and N are 71.04%, 16.83% and 12.13%, respectively. In Fig. S4b,† the peaks of C–C (284.8 eV), C–O (286.0 eV), C–N (287.7 eV) and O–C
O (288.9 eV) are observed in the high-resolution C 1s of CPDs. In high-resolution N 1s, the peaks of –NH2 (398.9 eV), pyrrolic N (400.3 eV) and graphite N (401.9 eV) are observed (Fig. S4c†). As shown in Fig. S4d,† O 1s analysis reveals three different types of oxygen atoms: C–O (531.0 eV), O–H (531.9 eV) and C
O (533.3 eV). These results confirm the presence of abundant functional groups, especially the carbonyl groups and N-containing groups, on the surface of CPDs.
A smooth surface of CC is clearly visible from the scanning electron microscopy (SEM) image, as illustrated in Fig. 1a. It is shown that there are some interval gaps and pores that exist on the CC (Fig. S5†). After GO is coated on CC through an easy wetting operation (denoted as GO-CC), the color of CC changes from white to dark brown, confirming the successful synthesis of GO-CC (Fig. 1i). Reduced graphene oxide was coated on cotton cloth by treating GO-CC in ammonia after annealing, where GO was converted into rGO and CC was partially graphitized (denoted as GCC). 700 °C is the optimized reaction temperature for the annealing treatment (Fig. S6†). As compared with CC, the annealed GCC has typical graphene folds with a rough surface as shown in Fig. 1b, in which rGO is uniformly distributed. The SEM elemental mapping image of GCC is shown in Fig. S7,† showing that C and O elements are homogeneously distributed in GCC.
![]() | ||
Fig. 1 (a–c) SEM images of CC, GCC and CPDs-GCC. (d) TEM image of CPDs-GCC. (e–h) SEM elemental mapping images of CPDs-GCC. (i) Digital photographs. |
CPDs-GCC was synthesized through simple solution immersion. No distinct morphology change is observed on the SEM images of GCC and CPDs-GCC (Fig. 1c), and the CPD-GCC substrate maintains the 3D structure of CC and GCC (Fig. S8 and S9†). Additionally, each treatment step leaves the cloth flexible, making it possible for the substrate to be folded and coiled into various forms without compromising its structural strength (Fig. 1i). As shown in Fig. 1d, CPDs are obviously identified in the TEM image, confirming their uniform distribution. The consistent distribution of C, O, and N elements in CPDs-GCC is evident in Fig. 1e–h. Compared with the mapping of GCC (Fig. S7†), the presence of N elements in CPDs-GCC is attributed to the CPDs.
Confocal laser scanning microscopy (CLSM) is used to clearly demonstrate the existence of CPDs due to the common fluorescent nature of carbon dots (Fig. S10†). After deposition, there is an obvious fluorescent signal on the fiber of CPDs-GCC, which clearly shows a homogeneous distribution in Fig. 2d–f. No fluorescent signal is found on GCC as expected in Fig. 2a–c. The above result suggests that these CPDs are tightly grown on the surface of GCC.
In connection with XPS, the surface information of CPDs-GCC is also ascertained. The major elements on the surface of CPDs-GCC are C, N and O (Fig. S11†). Compared to GCC (Fig. S12†), the CPD-GCC surface has nitrogen that is not present on GCC, and the percentage of oxygen increases from 8.93 to 32.4 at% (Tables S2 and S3†). The increase of N and O atoms originates from the CPDs attached to the surface of CPDs-GCC. The C–C, C–N, and O–CO peaks in the C 1s spectrum are located at 284.86 eV, 287.47 eV, and 288.44 eV, respectively (Fig. 2g). The N 1s signals are composed of three peaks at 400.72 eV, 402.58 eV and 403.72 eV, which correspond to the pyrrolic N, graphitic N and N–O bonds, respectively (Fig. 2h). As shown in Fig. 2i, O 1s signals are deconvoluted into three peaks at 532.33 eV, 533.69 eV and 534.99 eV, which correspond to the C–O, N–O and O–C
O, respectively. An obvious change in XPS spectra confirms that CPDs alter the chemical environment of the material by introducing N-containing groups and O-containing groups on the surface.
To investigate the mechanism behind the dendrite-free lithium deposition behavior on CPDs-GCC, we calculated the interaction energies between Li+ and the most abundant functional groups on CPDs, namely pyrrolic N and carboxyl (–COOH) groups. Density functional theory (DFT) calculations revealed that the binding energy between Li and the CO in –COOH is −2.38 eV, while that between Li and pyrrolic N is −2.76 eV, both significantly higher than the binding energy between Li and the C–C bonds in GCC (Fig. 3a and b).27 These higher binding energies indicate that the abundant functional groups on CPDs serve as active adsorption sites for Li, thereby reducing the nucleation energy barrier for Li deposition. To experimentally verify the interaction between Li and the functional groups, XPS was performed on the CPD-GCC anode after depositing 8 mAh cm−2 of Li (Fig. 3c). Deconvolution of the Li 1s spectrum yielded four peaks: the peak at 54.3 eV corresponds to metallic Li, while the peaks at 55.0 eV and 55.8 eV are attributed to O–Li bonds (from carbonyl groups) and Li–N bonds (from pyrrolic N), respectively. The peak at 56.8 eV corresponds to Li–F species, originating from the LiTFSI in the electrolyte. These results confirm the chemical interactions between Li and the pyrrolic N and carboxyl groups on CPDs, consistent with the DFT predictions. Moreover, similar results were observed after 20 cycles, further confirming the stability of these lithiophilic functional groups (Fig. S15†).
To further elucidate the role of functional groups in Li deposition behavior, COMSOL simulations were performed to model the Li+ concentration field near the electrode surface. Due to the poor lithiophilicity of GCC, a steep Li+ concentration gradient developed at its surface, leading to uneven deposition and the formation of dendritic protrusions over time (Fig. 3d). In contrast, the incorporation of CPDs significantly mitigated the concentration gradient at the CPD-GCC surface, effectively suppressing dendrite growth and promoting uniform Li+ deposition (Fig. 3e). This indicates that the addition of a CPD functional group can effectively inhibit the development and expansion of Li dendrites (Fig. 3f and g).
The deposition morphology on the bare Cu electrode and CPDs-GCC electrode during Li plating was also tested in open cells (Fig. S16†). After 5 min of plating, dendrites nucleate on the surface of Cu foil. The size of the dendrites grows as the plating progresses, while the surface morphology of CPDs-GCC does not change noticeably in the whole process of plating. Therefore, the CPD-GCC current collector mitigates the deadly problem of dendritic development.
The amount of CPDs added has also been explored. Various quantities of CPDs were dispersed to generate an aqueous solution (40 mg, 70 mg and 100 mg of CPDs were distributed in 10 mL of deionized water), and GCC samples were submerged in the three different aqueous solutions, respectively, denoted as 40 mg CPDs-GCC, 70 mg CPDs-GCC and 100 mg CPDs-GCC. The results reveal that 70 mg CPD-GCC cycled stably for more than 200 cycles with a CE of more than 97%, but 40 mg CPDs-GCC and 100 mg CPDs-GCC suffer a catastrophic short circuit after 80 and 40 cycles, respectively (Fig. S19†).
Furthermore, to clarify Li deposition behavior, a thorough investigation of voltage polarization was conducted. Fig. 4b shows a comparison of the Li plating voltage profiles on the CC, GCC, and CPDs-GCC. There is a noticeable voltage decrease when Li deposits on the material, and then a level voltage plateau follows. The Li metal nucleation overpotential is defined as the difference between the bottom of the voltage drop and the flat part of its plateau, which is mostly determined by the properties of the substrate. The nucleation potential of the CC was about 48 mV, which is much higher than the nucleation potentials of the GCC (21 mV) and CPDs-GCC (13 mV). The minimal nucleation overpotential of the CPDs-GCC is in accordance with uniform Li nucleation.
Galvanostatic cycling performance was used to evaluate the voltage hysteresis and long-term cycling stability of the anode (with Li foil as the counter electrode). The cycling stability of CPDs-GCC is maintained up to 3400 h at 2 mA cm−2 and 1 mAh cm−2, while a short circuit occurs in GCC symmetric cells after 2850 h (Fig. 4c). For a certain current density of 2 mA cm−2 at 3 mAh cm−2, these three types of symmetric coin cells were operated (Fig. 4d). Markedly, the CPD-GCC cell displays a stable voltage profile and an incredibly long lifespan of 4800 h, which is either better than or equal to the results that have been previously reported (Table S4†). In contrast, the GCC cell shows a fluctuant voltage profile with substantially greater voltage polarization, and CC exhibits a short circuit after 100 h. Moreover, CPDs-GCC exhibits a higher Li+ transference number. Compared with that of GCC (0.692, Fig. 4e), the Li+ transference number of CPDs-GCC reaches as high as 0.781 (Fig. 4g). Fig. 4f and h show the electrochemical impedance spectra of the GCC cell and the CPDs-GCC cell before and after the it test. Notably, the half-cell assembled with the CPD-GCC anode demonstrates remarkably low voltage hysteresis and rapid ion kinetics during galvanostatic charge–discharge cycling. This intriguing performance prompted us to investigate the underlying mechanisms in detail.
Therefore, the voltage hysteresis is primarily governed by the distribution of the ionic concentration field, the diffusion/transport rate of Li+ ions, and the interfacial reaction kinetics. As demonstrated in Fig. 3d and e, the presence of lithiophilic functional groups on the CPDs leads to a more uniform Li+ distribution and a smaller ionic concentration gradient on the CPD-GCC electrode surface. To further investigate the ion diffusion kinetics, we simulated the migration behavior of Li+ ions on the surfaces of GCC and CPD-GCC electrodes (Fig. 5a and c). The Li+ migration energy barrier on CPDs-GCC (0.22 eV) is significantly lower than that on GCC (0.35 eV), indicating that Li+ ions migrate more easily on the CPD-GCC surface. As a result, at the same current density, the local ionic concentration on CPDs-GCC is lower than that on GCC. The chronoamperometry (CA) test further supports this conclusion, showing that Li+ ions quickly enter a 3D diffusion regime on the CPD-GCC surface (Fig. 5d).
Additionally, symmetric cells were assembled using GCC//GCC and CPD-GCC//CPD-GCC configurations (without lithium deposition) to evaluate the ionic conductivity of the electrodes. As shown in Fig. 5e, the CPD-GCC electrode exhibits higher ionic conductivity than GCC. These findings collectively confirm that both on the electrode surface and within the bulk, Li+ ions in CPDs-GCC can transport more rapidly, leading to a more uniform Li+ concentration field.
Subsequently, we investigated the interfacial reaction kinetics. Electrochemical impedance spectroscopy (EIS) was conducted at various temperatures to calculate the activation energy for Li+ interfacial charge transfer on both electrodes (Fig. S20†). As illustrated in Fig. 5f, the activation energy on CPDs-GCC is 17.37 kJ mol−1, markedly lower than that on GCC (29.93 kJ mol−1), indicating a faster interfacial reaction rate for Li+ on CPDs-GCC. The time–voltage profiles of symmetric cells at different current densities were further evaluated. As the current density increased from 1 to 5 mA cm−2, the voltage hysteresis increased accordingly. Compared with GCC, the CPD-GCC anode cell exhibits a lower voltage hysteresis, which can be attributed to the accelerated ion transport and interfacial reaction kinetics (Fig. 5g).
Additionally, we calculated the exchange current density (i0) for both materials, as shown in the following equation:
Here, i represents the current density, F is the Faraday constant, R is the gas constant, T is the temperature, and η denotes the voltage hysteresis of the battery (Fig. 5h). Linear fitting analysis reveals that CPDs-GCC (i0 = 3.211 mA cm−2) exhibits a higher exchange current density compared to GCC (i0 = 2.423 mA cm−2) (Fig. 5i). This indicates that the lithiophilic functional groups of the CPDs accelerate the interfacial reaction kinetics of Li+.
In summary, we believe that the introduction of lithiophilic functional groups on CPDs-GCC is the key factor enabling the electrode to exhibit an ultralow voltage hysteresis of 2 mV. Compared with GCC, Li+ ions arriving at the electrode surface are rapidly dispersed due to the interaction with lithiophilic sites, which effectively reduces the local ion concentration. Meanwhile, at the electrode–electrolyte interface, Li+ ions are quickly reduced and deposited, promptly consuming the accumulated Li+ at the surface. This synergistic effect of enhanced surface diffusion and accelerated interfacial reaction results in ultralow voltage hysteresis maintained throughout long-term cycling.
To further illustrate the practical utilization of the available flexibility of the CPD-GCC anode, a LiFePO4 cathode/separator/CPD-GCC anode was employed for building a pouch cell. To seal the electrodes, two thin sheets of aluminum plastic film were employed, which had a surface area of roughly 3 × 3 cm2. A flexible pouch cell (FPC) exhibits an initial voltage of 3.03 V, and it does not change even when bent, which demonstrates that the battery is both flexible and stable (Fig. 6d). The voltage of two FPCs in series is 5.97 V, demonstrating the feasibility of the method of connecting in series to provide higher voltages for electronic devices (Fig. S21†). Noticeably, a CPDs-GCC FPC powers two separate LEDs under both flat and bending conditions, indicating a possible application in flexible wearable electric devices (Fig. 6e and f).
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d5gc02081f |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2025 |