Zhandong
Ren
*a,
Zhiqiang
Xie
a,
Li
Deng
a,
Chen
Dong
a,
Guocan
Song
a,
Xiaohui
Liu
a,
Juanjuan
Han
a,
Lin
Zhuang
b,
Yi
Liu
c and
Yuchan
Zhu
*a
aSchool of Chemical and Environmental Engineering, Wuhan Polytechnic University, Wuhan, 430023, P. R. China. E-mail: renzhandong@163.com; zhuyuchan@163.com
bCollege of Chemistry and Molecular Sciences, Hubei Key Lab of Electrochemical Power Sources, Wuhan University, Wuhan, 430072, P. R. China
cState Key Laboratory of Separation Membranes and Membrane Processes, School of Chemistry, Tiangong University, Tianjin 300387, P. R. China
First published on 29th August 2023
Water electrolysis is the most fascinating procedure for producing pure hydrogen owing to its flexibility and convenience. Platinum (Pt) is the most effective electrocatalyst for the hydrogen evolution reaction (HER) but its high price and scarcity have greatly restricted its commercial application. Therefore, it is necessary to greatly increase the mass activity (MA) of Pt to meet practical applications. In the present study, an oxidized Pt atomic cluster-supported Au electrode (PtAC–O–Au) with an ultra-low loading was prepared by high vacuum magnetron sputtering combined with electrochemical anodic oxidation. The (PtAC–O–Au)-1 electrode has a very high mass activity (MA), reaching 49.2 A mgPt−1 at an overpotential of 50 mV, which is 41 times that of the 20 wt% Pt/C electrode and 20 times that of the 0.5 wt% Pt/C electrode. Even at such a low load, the (PtAC–O–Au)-1 electrode has excellent apparent activity and only needs an overpotential of 41 mV@10 mA cm−2, which is close to that of the 20 wt% Pt/C electrode (37 mV@10 mA cm−2). Moreover, the (PtAC–O–Au)-1 electrode has an ultra-high specific activity (SA). The SA of (PtAC–O–Au)-1 is 12–18 times higher than that of the 0.5 wt% Pt/C electrode and 36–56 times higher than commercial Pt/C electrodes. More importantly, it was confirmed by the electrochemical analysis method (cyclic voltammetry and CO adsorption–stripping) and X-ray photoelectron spectroscopy (XPS) that the active site is the oxidized platinum (Pt–O–Au) on the surface of the electrode. Density functional theory (DFT) calculations have also elucidated that the absolute value of ΔGH*(Pt) of PtAC–O–Au is close to that of Pt(111), indicating that its outstanding HER activity originates from its optimal ΔGH*(Pt) value.
In terms of Pt loading, although there have been good achievements, it is still necessary to further reduce the loading. Some electrocatalysts with low Pt loadings have been developed, such as PtW NPs/C,36 Pt3Ni2 NWs–S/C,42 Pt–MoS2,43 Pt/def-WO3@CFC,44 Pt@MoS2/NiS2,45 Mo2TiC2Tx–PtSA,46 Pt–MoO2@PC,47 and so on. However, the Pt loading in the above-mentioned electrocatalysts has exceeded 10 μg cm−2. Further research results have reduced the Pt loading to less than 10 μg cm−2, such as Pt5/HMCS,11 Pt Cs/MoO2 NSs-L,16 CNT/Pt@CdSe-OCPs,30 AL-Pt/Pd3Pb,37 Pt-GT-1,48 CDs/Pt–PANI,49 Pt@mh-3D MXene,50 Pt–GDY-2,51 Pt–HNCNT,52 Pt–Ru dimer,53etc. To date, little research has been done on the Pt loading of less than 1.0 μg cm−2, except for Pt SA/m-WO3−x,17 Pt/TiBxOy,21 Pt–ACs/CoNC,54 PtOx/TiO2,55 and Pt–SAs/WS256 electrocatalysts. Most of these studies have revealed the HER activity of metallic Pt. However, some interesting phenomena regarding the oxidized Pt still require detailed attention.54–60 Therefore, the purpose of this study is to study the HER activity of oxidized Pt at very low loading (<1.0 μgPt cm−2).
To obtain the ultra-low Pt electrode, the high vacuum magnetron sputtering method has been adopted in this study. The magnetron sputtering can uniformly deposit metal elements on the substrate surface in the form of atomic clusters, which can realize ultra-low load deposition through the control of the sputtering process. However, there are few applications in the preparation of electrode materials at present.61–63 The Pt loading of the (PtAC–O–Au)-1 electrode (0.48 μgPt cm−2) is much lower than the Pt loading in most reports (Table S3 (ESI†)). Through characterization analysis, it has been proved that Pt atomic clusters (PtAC) with a particle size of 0.8 nm can be deposited on the surface of the Au underlayer under the low power and high vacuum magnetron sputtering. Moreover, the Au underlayer has the characteristic of specific growth along the [111] direction. More importantly, it has been confirmed that a new and stable active site is formed on the surface of the electrode after the electrochemical oxidation. The combination of X-ray photoelectron spectroscopy (XPS) and electrochemical analysis methods (cyclic voltammetry and CO adsorption–stripping) has suggested that the active site should come from the oxidized platinum (Pt–O). In addition, density functional theory (DFT) calculations have elucidated that the ΔGH*(Pt) (absolute value) of PtAC–O–Au is close to that of Pt(111), indicating that its outstanding HER activity originates from its optimal ΔGH* value. The (PtAC–O–Au)-1 electrode not only possesses ultra-high MA as compared with the commercial Pt/C with the same loading (0.5 μgPt cm−2) but also possesses the apparent activity equivalent to the commercial 20 wt% or 40 wt% Pt/C with high loading.
PtAC–O–Au has the morphology of atomic clusters, a special crystal structure and a modified electronic structure. First, for the Au underlayer, the size of Au nanoparticles can be seen, with an average particle size of 26.8 nm (Fig. S1 and S2 (ESI†)). Fig. 1a is an AFM image of (PtAC–Au)-1, in which the particle distribution is relatively uniform. The mean particle diameter of PtAC–Au slightly increased with the enhancement of Pt loading, ranging from 28.4 ((PtAC–Au)-1, 0.482 μg cm−2) to 31.4 nm ((PtAC–Au)-4, 1.693 μg cm−2) (Fig. S1 and S2 (ESI†)). Therefore the particle size of Pt atomic clusters sputtered in the subsequent process is small, which has no significant effect on the particle size of the Au underlayer. Moreover, the analysis of the surface roughness of PtAC–Au revealed that the surface flatness was improved after loading the Pt atomic clusters. The height difference for pure Au was 7.5 nm, while the height differences for (PtAC–Au)-1, (PtAC–Au)-2, (PtAC–Au)-3 and (PtAC–Au)-4 were reduced to 6.2, 5.7, 5.2 and 4.3 nm, respectively (Fig. S3 (ESI†)). The root-mean-square roughness (Rq) of Au was 2.91 nm, while the Rq of (PtAC–Au)-1, (PtAC–Au)-2, (PtAC–Au)-3 and (PtAC–Au)-4 dropped to 2.88, 2.77, 2.65 and 2.40 nm, respectively. The decrease in the height difference and Rq indicated that the electrode surface became smooth. It may be that the fine Pt atomic clusters were filled into the gaps of the large Au particles, thereby improving the flatness of the electrode.
The HRTEM image of (PtAC–Au)-1 (Fig. 1b) facilitated the investigation of the lattice fringes of Au(111) and Au(200) but no lattice fringes of Pt were found. It was presumed that Pt exists in the form of an amorphous phase or atomic cluster. The particle size distribution of (PtAC–Au)-1 was uniform, based on the TEM images (Fig. S4 (ESI†)), which is consistent with the AFM observation results. Moreover, in the STEM-EDS elemental mapping (Fig. 1c), the distribution of Au and Pt elements was uniform. The (PtAC–Au)-1 electrode was anodized at a potential of 1.7 V for 10 min to obtain a stable (PtAC–O–Au)-1 electrode (Fig. S5 (ESI†)). In the HRTEM diagram (Fig. 1e), the lattice stripes of Au(111) and Au2O3(111) can be seen, where the generation of Au2O3 is mainly derived from the anodic oxidation process. Au and Pt are distributed evenly in the STEM-EDS elemental maps and the particle size distribution was also uniform, as observed from the HAADF-STEM image (Fig. 1f). Since the particle size of Pt is significantly less than that of Au, it is difficult to accurately observe the particle size and lattice stripe of Pt particles in Fig. 1e. Therefore, the HAADF-STEM and HRTEM analyses of Pt-1 ((PtAC–Au)-1 without Au underlayer) were performed and the results are shown in Fig. 1d. The Pt cluster is very small, only about 0.89 nm and it can be seen from the STEM diagram that the particle size distribution of Pt particles is uniform (Fig. S6 (ESI†)). After careful examination of the HRTEM image of Pt-1 (Fig. S6 (ESI†)), the lattice fringes of the Pt(111) crystal plane were observed, although most Pt particles were in the amorphous state. With the increase in sputtering time, the Pt loading increased. For example, the Pt load of the (PtAC–Au)-4 electrode was 6 times that of the (PtAC–Au)-1 electrode. For the (PtAC–Au)-4 electrode, the Pt crystal stripes were observed around Au nanoparticles even though there were also many amorphous stripes (Fig. S7 (ESI†)).
The special crystal structure of the PtAC–O–Au is analyzed in Fig. 1g and S8 (ESI†). The characteristic diffraction peaks of the (111) and (200) crystal facets of Au were observed at 38.2° and 44.4° for (PtAC–O–Au)-1 in Fig. 1g. Since the Pt loadings are very low, no diffraction peaks of Pt were observed for (PtAC–O–Au)-1, (PtAC–O–Au)-2, (PtAC–O–Au)-3 and (PtAC–O–Au)-4 (Fig. S8 (ESI†)). Only for the (PtAC–O–Au)-5 (the Pt loading = 17.58 μgPt cm−2) can the (111) crystal plane of Pt can be seen in the XRD diffraction pattern. The intensity ratio of the diffraction peaks of (111) and (200) crystal planes is about 30:1 for the (PtAC–O–Au)-1, which is far from the data from JCPDS 04-0784, indicating that the crystal structure is dominated by the [111] crystal orientation; this may be due to the preparation methods. In the magnetron sputtering technique, the sputtering power will affect the orientation of the planes of the metal. When the sputtering power is low, the close-packed plane crystal at low energy is preferentially formed. This kind of electrode with specific growth along a certain crystal direction is more convenient to coincide with the stable crystal surface selected by theoretical calculation, so we attribute this special electrode morphology to the model electrode.
The loading of Pt was investigated by ICP-OES, EDS and XPS. The elemental analysis results of (PtAC–O–Au)-1 demonstrated that the Pt content was very low (ICP-OES: 0.5 atom%; EDS: 1.5 atom%; XPS: 4.8 atom%) (Fig. 1g (inset) and Fig. S9 (ESI†)). The Pt loading increased from 0.482 to 1.693 μgPt cm−2 with sputtering time, showing a good linear correlation (Table S1 and Fig. S10 (ESI†)). The proportion of Pt in the PtAC–O–Au surface analyzed by XPS was higher than that obtained by ICP-OES. With the increase of sputtering time, the Pt content on the electrode surface increased from 4.79 to 42.4 atom% (Table S2 (ESI†)). This ratio is much higher than that of Pt in the body, indicating that Pt is highly dispersed in the electrode surface layer.
Fig. 1h and i are the electronic structure analyses of Pt and Au on the surface of the (PtAC–O–Au)-1. The survey XPS spectra of the Au, Pt-2 and (PtAC–O–Au)-1 demonstrate the presence of Pt, Au, O and C species (Fig. S11 (ESI†)). The Pt element of the Pt-2 surface mainly exists in Pt0+ and Pt2+ components in Fig. 1h. The two peaks at the binding energies of 71.3 and 74.5 eV correspond to the 4f7/2 and 4f5/2 orbitals of Pt0+ species, while the two peaks at 72.2 and 75.5 eV are attributed to the 4f7/2 and 4f5/2 orbitals of Pt2+ species. However, for (PtAC–O–Au)-1, only the Pt4+ components (74.9 and 78.3 eV)54 appeared on the surface and almost no Pt0+ components were found. In addition, the binding energies of Au 4f of the PtAC–O–Au electrode were at 84.4 and 88.1 eV (Au: 84.0 and 87.7 eV),64 indicating that the partial oxidation of Au also occurs on the surface of PtAC–O–Au.
The HER activities of (PtAC–O–Au)-1, Pt-1 and 0.5 wt% Pt/C electrodes are displayed in Fig. 2a. To ensure the fairness of the evaluation, the Pt loading of all electrodes was controlled at about 0.5 μg cm−2. The Pt-1 and 0.5 wt% Pt/C electrodes do not exhibit excellent HER activity because of their ultra-low loading of Pt. However, the (PtAC–O–Au)-1 electrode exhibited excellent HER activity, which was not affected by its low Pt loading. For instance, the overpotential at 10 mA cm−2 (η10) was 140 mV and 168 mV for the Pt-1 and 0.5 wt% Pt/C electrodes, respectively, while the η10 of the (PtAC–O–Au)-1 electrode was only 41 mV. At the same time, the pure Au electrode did not show any HER activity in the investigated potential range. The HER activity of the (PtAC–O–Au)-1 electrode was further compared with those of the commercial Pt/C catalyst (40 wt% Pt/C (40 μgPt cm−2) and 20 wt% Pt/C (20 μgPt cm−2)) electrodes (Fig. 2b). The HER activity of the (PtAC–O–Au)-1 electrode was significantly higher than that of the 20 wt% Pt/C, similar to those of 40 wt% Pt/C electrodes.
For the noble metal Pt, the mass activity (MA) is very important, which is related to the actual usage of the noble metal. However, the comparison of MA in most reports is at present incomplete. This is because it is unreasonable to compare MA for low-load Pt catalysts and high-load commercial Pt/C alone. The Pt load of commercial Pt/C is very high (tens or hundreds of times higher than that of low-load Pt catalyst), and the deviation of the apparent activity according to mass standardization is very large. The research results of ref. 11 have already illustrated similar conclusions. Therefore, to correctly evaluate the MA of Pt catalysts with low loads, it was necessary to supplement the MA of commercial Pt/C catalysts with similar loads. The MAs of all the electrodes at different overpotentials (20, 50 and 80 mV) are shown in Fig. 2c and d. The (PtAC–O–Au)-1 electrode exhibited an ultra-high MA (3.0 A mg−1@η = 20 mV; 49.2 A mg−1@η = 50 mV; 329.0 A mg−1@η = 80 mV). The MA of the (PtAC–O–Au)-1 electrode is 20–22 times higher than that of the Pt-1 and 0.5 wt% Pt/C electrodes at η of 50 mV. The MA of the (PtAC–O–Au)-1 electrode is 60–66 times higher than that of the Pt-1 and 0.5 wt% Pt/C electrodes at the η of 80 mV. For the commercial Pt/C electrodes (20 wt% and 40 wt%), the MA is 26–41 times lower than that of (PtAC–O–Au)-1 electrode at η of 50 mV. More importantly, the MA of the (PtAC–O–Au)-1 electrode is significantly higher than that in most reports (Table S3 (ESI†)). The apparent activity depends on the electrochemical surface area (ECSA) of the electrocatalyst. The high Pt loading of the commercial Pt/C catalyst and the porous structure of the activated carbon support can make Pt highly dispersed, thus showing a great ECSA (30.8 and 15.2 cm2 in Fig. S12e and f (ESI†)). Although the Pt-2 electrode has no abundant pore structure, its high loading capacity allows its ECSA to still reach 3.09 cm2, which is 10 times larger than that of the (PtAC–O–Au)-1 electrode (Fig. S12d (ESI†)). For the (PtAC–O–Au)-1 electrode, despite the tiny particle size and high dispersion obtained by magnetron sputtering, its ECSA is very small due to its ultra-low loading (0.264 cm2 in Fig. S12b (ESI†)). The low ECSA (for the same reason) also occurs on the Pt-1 and 0.5 wt% Pt/C electrodes (Fig. S12a and c (ESI†)). The ECSA of the (PtAC–O–Au)-1 electrode is only 0.85–1.7% of the commercial Pt/C electrodes and 8.5% of the Pt-2 electrode. For the specific activity (SA), the normalized current of the commercial Pt/C (20 wt% and 40 wt%) is very low (Fig. S13†). The SAs of 0.5 wt% Pt/C and Pt-1 electrodes are relatively close (Fig. 2e) but their SAs are much lower than that of the (PtAC–O–Au)-1 electrode. The SA of the (PtAC–O–Au)-1 electrode is 12–18 times higher than that of Pt-1 and 0.5 wt% Pt/C electrodes and 36–56 times higher than that of the commercial Pt/C electrodes. Therefore, both the MA and SA of the (PtAC–O–Au)-1 electrode were greatly improved. The reason for the increase in the MA and SA activities of the HER is not only the extremely low utilization rate of Pt but also the improvement of the turnover frequency (TOF) of active sites. The TOF of the (PtAC–O–Au)-1, 0.5 wt% Pt/C and Pt-1 electrodes are shown in Fig. S14,† in which the (PtAC–O–Au)-1 electrode shows significantly increased HER activity.
The mechanism of the HER reaction was further analyzed by the Tafel slope in Fig. 2f. The Tafel slope of the (PtAC–O–Au)-1 electrode was significantly lower than that of the Pt-1 and 0.5 wt% Pt/C electrodes. The Tafel slope of the (PtAC–O–Au)-1 electrode was 28.6 mV dec−1, indicating that the reaction mechanism is the Volmer–Tafel process and the rate-determining step is the combination desorption of Had (Had + Had = H2). For the Pt-1 and 0.5 wt% Pt/C electrodes, the rate-determining step is the Heyrovsky step (H3O+ + Had + e− = H2 + H2O), according to the slope.65 The difference in the reaction mechanism determines the difference in reactivity between them.
Further attempts were made to appropriately increase the Pt loading of the PtAC–O–Au electrodes. With the continuous increase in the Pt loading, their HER activities also increased slightly. Among them, the apparent current densities of the (PtAC–O–Au)-2, (PtAC–O–Au)-3 and (PtAC–O–Au)-4 electrodes exceeded that of the Pt-2 electrode (Fig. S15a (ESI†)). It was further demonstrated that the PtAC–O–Au electrode is a very good HER electrocatalyst. The increase in the HER activity may be related to the ECSA enhancement (ECSA((PtAC–O–Au)-1) = 0.264 cm2; ECSA((PtAC–O–Au)-2) = 0.604 cm2; ECSA((PtAC–O–Au)-3) = 1.023 cm2; ECSA((PtAC–O–Au)-4) = 1.4 cm2 in Fig. S16 (ESI†)). The HER activity was further normalized by the ECSA (Fig. S15b (ESI†)). The SAs are of the order of (PtAC–O–Au)-1 > (PtAC–O–Au)-2 > (PtAC–O–Au)-3 > (PtAC–O–Au)-4. Moreover, the SAs are all much higher than that of the Pt-2 electrode. For the MA, the order is the same (Fig. S15c (ESI†)). It can be predicted that the active site of the PtAC–O–Au electrode is not necessarily on the surface of an ordinary Pt atom. It may not be reasonable to normalize the HER current with the ECSA of Pt, which will be further analyzed in detail later.
The excellent HER activity of the PtAC–O–Au electrode may be related to the surface oxidation process.66 The apparent activity of the (PtAC–Au)-1 electrode is not good enough without the anodic oxidation (Fig. S17a (ESI†)). After anodic oxidation at 1.7 V for 10 min, the apparent activity of the (PtAC–O–Au)-1 electrode increased. For instance, the η10 was 152 mV for the (PtAC–Au)-1 electrode, while the η10 of the (PtAC–O–Au)-1 electrode was only 41 mV. The enhancement in activity was not only due to the oxidation of Au because the apparent activity of the AuOx electrode was not significantly improved (Fig. S17a (ESI†)). Meanwhile, the increase in activity was not entirely from the PtOx since the apparent activity of the PtOx-1 electrode was still poor (Fig. S17a (ESI†)). Only when Au and Pt were oxidized together to form the band of Pt–O–Au could the apparent activity be remarkably improved. Therefore, the oxidation process should play an important role and needs to be studied in detail.
In the oxidation potential range of 0.7–1.1 V, the obvious underpotential deposition of H (H-UPD) and HER currents cannot be generated (Fig. 3a). When the oxidation potential increased to 1.3 V, the H-UPD and HER currents appeared at 0.2 and 0 V (0.12 mA cm−2). Once the oxidation potential was further increased to 1.5 and 1.7 V, the obvious HER current increased to 0.18 mA cm−2. Moreover, in Fig. S17b and c (ESI†), the apparent activity of (PtAC–O–Au)-1 at the anodic oxidation potential of 1.7 V was higher than that of 1.3 V. The above results have demonstrated that only when the electrode surface is completely oxidized at 1.7 V will its HER activity be significantly increased.
It was also found that when the oxidation potential was higher than 1.3 V, three reduction peaks (▲, ★, ●) appeared during the negative scanning of the potential (Fig. 3a). One belongs to the reduction peak of Au–OH (▲, 1.12 V) and the other belongs to the reduction peak of Pt–OH (●, 0.62 V). However, the reduction peak at 0.72 V (★, star peak) needs further study to determine its origin. To accurately determine the origin of the reduction peak at 0.72 V, the LSV curves of pure Au electrode oxidized at different potentials were analyzed in detail (Fig. 3b). Regardless of whether the oxidation potential is increased to 1.5 V or 1.7 V, there was no obvious “star peak”. Thus, it can be concluded that the “star peak” is not the reduction peak of Au–OH. Further analysis was carried out in the CVs of PtAC–O–Au electrodes with different Pt loadings (Fig. 3c). With the increase in the Pt loading, the reduction current at 0.62 V increased, while the reduction current of the “star peak” did not change. This indicates that the “star peak” is not due to the reduction of Pt–OH. Therefore, the “star peak” is the reduction peak for neither Au–OH nor Pt–OH. Since the “star peak” is just between the Au–OH and Pt–OH reduction peaks, it is speculated that it is the reduction peak of the newly formed “Pt–O–Au” active site in the electrochemical oxidation process, which can efficiently adsorb and desorb H atoms. Therefore, the HER apparent current was further normalized by the ECSA derived from the capacitance of the “star peak” (Fig. S18 (ESI†)), which has shown that the SA of HER is essentially the same (Fig. S19 (ESI†)), indicating that the active site is located in “Pt–O–Au” at 0.72 V (★, star peak).
The electronic structures of PtAC–Au and PtAC–O–Au electrodes were further analyzed (Fig. 3d–f and Fig. S20 (ESI†)). The Pt electronic structure of the (PtAC–Au)-1 electrode surface was mainly Pt0+ and Pt2+ components (Fig. 3d). The two peaks at binding energies of 71.5 and 74.6 eV correspond to the 4f7/2 and 4f5/2 orbitals of Pt0+, while the two peaks at 72.2 and 75.4 eV were attributed to the 4f7/2 and 4f5/2 orbitals of Pt2+, respectively. After the anodic oxidation, the Pt4+ components (74.9 and 78.3 eV) appeared on the (PtAC–O–Au)-1 electrode surface, while Pt0+ components were significantly reduced. Meanwhile, the Au in the (PtAC–O–Au)-1 electrode was partially oxidized to form AuOx, while it was Au0+ in the (PtAC–Au)-1 electrode (Fig. 3e). When the Pt load increased, the binding energy peak of Pt4+ 4f5/2 exhibited a significant negative shift (78.47 eV for the (PtAC–O–Au)-1, 78.09 eV for the (PtAC–O–Au)-3, 77.85 eV for the (PtAC–O–Au)-4 and 77.69 eV for the (PtAC–O–Au)-5 in Fig. 3f), indicating that the valence state of Pt decreased. At the same time, the number of Pt4+ components also decreased significantly with the increase in the Pt loading. Pt4+ rarely appears on the surfaces of the pure Pt-2 electrode (Fig. S21 (ESI†)); therefore, it indicates that the Pt4+ valence state of the (PtAC–O–Au)-1 electrode is at the interface between the Pt and Au atom (Pt–O–Au). The Pt loading in the (PtAC–O–Au)-5 electrode is 36.5 times that in the (PtAC–O–Au)-1 electrode and there is almost no exposed Au–Pt interface on the electrode surface, so Pt4+ rarely appears (Fig. S21 (ESI†)). Correspondingly, the anodic oxidation of Au was inhibited as the Pt loading increased. This is reflected in the negative shift of the Au 4f binding energy of the (PtAC–O–Au)-4 electrode as compared to the (PtAC–O–Au)-1 electrode or (PtAC–O–Au)-3 electrode (Fig. S22 (ESI†)). In addition, the oxidation state of the (PtAC–O–Au)-1 electrode was stable (Fig. 3d and e). After a long-term lifetime test, the valence states of Pt and Au in XPS graph remained unchanged, except for a small amount of oxidized Pt being converted into reduced Pt.
As can be seen from Fig. 4a, the CO adsorption–stripping curves of PtAC–O–Au electrodes with different Pt loadings are different. First of all, no obvious stripping peak was found on the surface of the AuOx electrode, which should correspond to the weak CO adsorption ability of AuOx. However, for the (PtAC–O–Au)-1 electrode, a clear stripping peak appeared at 1.15 V, which is attributed to the strong adsorption of CO on the surface of the electrode. The position of the stripping peak is different from that of the Pt-2 electrode (0.93 V), indicating that its adsorption active center is not just Pt. With the increase in the Pt loading, the peak potential negatively shifted to 1.0 V ((PtAC–O–Au)-2 electrode), 0.96 V ((PtAC–O–Au)-3 electrode) and 0.94 V ((PtAC–O–Au)-4 electrode), respectively; the peak area also increased, and the peak symmetry became better. In addition, during the anodic oxidation, there was no obvious peeling peak curve at the potential of 1.3 V. If the oxidation potential increased to 1.7 V, a sharp stripping peak appeared for the PtAC–O–Au electrode with different loads (Fig. S23 (ESI†)). This indicates that the anodic oxidation potential is also a very important factor. The potential of 1.7 V is generally considered the potential of the Au surface oxidation. Therefore, if the oxidation potential exceeds 1.7 V, it is possible to form Pt–O–Au active sites.
To further understand the extremely high HER activity of the PtAC–O–Au electrode, DFT calculations were carried out to investigate the Gibbs free energy of hydrogen adsorption (ΔGH*). It is a widely accepted descriptor in predicting the theoretical activity of the HER. A moderate ΔGH* should be around 0 eV, which would lead to the optimal HER activity due to the balance between the adsorption and the desorption steps. Therefore, the ΔGH* of H* adsorbed on different surface models including Au(111), Pt(111), Pt@PtAC–Au and Pt@PtAC–O–Au, as well as PtO2(111), were calculated in Fig. 4b and c. The ΔGH* of Pt(111) is −0.25 eV, which is consistent with the report in the literature.67 The Au(111) and PtO2(111) surfaces were 0.55 and −0.34 eV, respectively. The ΔGH* of the Pt@PtAC–Au surface was −0.42 eV, which is too negative, implying strong hydrogen adsorption. In contrast, the ΔGH* of the Pt@PtAC–O–Au surface increased to 0.28 eV, which is beneficial for the hydrogen desorption step. The above calculation results indicate that the ΔGH* (absolute value) of the Pt@PtAC–O–Au surface is close to that of Pt(111), indicating that its outstanding HER activity originates from its optimal ΔGH* value.
The EIS is a powerful, nondestructive and informative technique used extensively to study the electrolyte–electrode interfacial properties. The Nyquist diagrams of Au, (PtAC–Au)-1, (PtAC–O–Au)-1 and Pt-2 electrodes recorded at the overpotential of 50 mV are shown in Fig. 4d. The equivalent circuit corresponding to the EIS data was fitted with a two time-constant model (Rs(RfCf)(RctCdl)), which consists of the electrolyte solution resistance Rs, the electrode film resistance Rf, the charge transfer resistance Rct in series with a parallel connection of the film capacitance and double layer capacitance Cf and Cdl. The charge transfer resistance data were obtained in the low-frequency zone, which is related to the electrocatalytic kinetics. The Rct of the (PtAC–O–Au)-1 electrode is 1.437 Ω cm2, which is similar to that of the Pt-2 electrode (1.833 Ω cm2). It is also much lower than those of the Au (2208 Ω cm2) and (PtAC–Au)-1 (1818 Ω cm2) electrodes, suggesting fast charge transport during the HER process. For the solid electrodes, the double-layer capacitance is substituted by a constant phase element (CPE). Therefore, Cdl can be calculated and the surface roughness factor (Rf) can be calculated from the formula (Rf = Cdl/20 mF cm−2). The Rf values of four electrodes are both low and similar (Rf(Au) = 3.4, Rf((PtAC–Au)-1) = 1.5, Rf((PtAC–O–Au)-1) = 2.7, Rf(Pt-2) = 2.9), indicating that they all have smooth surfaces. Accelerated CV tests were conducted to investigate the stability of the catalysts in the potential range of −0.2 to 0.1 V at a sweeping rate of 50 mV s−1. The HER activity of the (PtAC–O–Au)-1 electrode was maintained without the slightest reduction after 2000 cycles of CV measurement in Fig. 4e. Additionally, the results of chronopotentiometry showed that the overpotential generally remains stable at a current density of 50 mA cm−2 over 20 hours in Fig. 4f. Under this current density, the overpotential increased by 8.6%, suggesting that the (PtAC–O–Au)-1 electrode is durable for hydrogen evolution.
Fig. 5 shows the new active site of “Pt–O–Au” of the PtAC–O–Au electrode. For the (PtAC–O–Au)-1 electrode, the Pt loading on the Au surface is very low and highly dispersed so Pt exists in the form of the +4 valence after electrochemical oxidation (the evidence comes from the XPS diagram). At the same time, the surface of Au was partially oxidized (the evidence comes from the XPS diagram), thus forming Pt–O–Au active sites. The electrochemical evidence of the Pt–O–Au active site corresponds to the reduction peak at 0.72 V (star peak) in the CV scan, which is different from the potential of the Pt–OH reduction peak (0.62 V). The SAs normalized by the ECSA derived from the capacitance of the “star peak” are essentially the same (Fig. S19 (ESI†)), indicating that the active site is located in “Pt–O–Au” at 0.72 V (star peak). The area ratio of the reduction peak of Pt–O–Au to the reduction peak of Pt–OH is 1.75:1, which indicates that most Pt exists in the form of Pt–O–Au active sites on the (PtAC–O–Au)-1 electrode. As for the (PtAC–O–Au)-4 electrode, with the increase in the Pt loading, its nucleation grows continuously so the active sites of Pt–O–Au are relatively fewer. The area ratio of the reduction peak of Pt–O–Au to the reduction peak of Pt–OH decreased to 1:9.7. Another electrochemical evidence that can prove the formation of new Pt–O–Au active sites comes from the CO stripping curves. The adsorption of CO on the Pt surface is very sensitive, and the subtle changes in the electrode surface can be reflected in the CO stripping curve. On the surface of (PtAC–O–Au)-4, the CO oxidation stripping potential of CO is 0.94 V, which is similar to that of pure Pt. On the surface of (PtAC–O–Au)-1, the potential of CO oxidation stripping is 1.15 V, which has an obvious offset. This shows that a new active site, Pt–O–Au, was formed on the (PtAC–O–Au)-1 surface, which is different from the pure Pt surface. The reason the above electrochemical analysis can clearly show the differences between different electrodes is also due to the electrode with a flat surface obtained by high vacuum magnetron sputtering technology in this experiment. This is different from the electrode material of porous carriers used in most electrocatalyst experiments at present. However, the improvement of the intrinsic activity of electrocatalysts can be reflected more truly and reasonably by using planar electrodes.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3qi01437a |