Hua-Zhong
Fan
,
Xing
Yang
,
Yan-Chen
Wu
,
Qing
Cao
,
Zhongzheng
Cai
* and
Jian-Bo
Zhu
*
National Engineering Laboratory of Eco-Friendly Polymeric Materials (Sichuan), College of Chemistry, Sichuan University, Chengdu 610064, People's Republic of China. E-mail: zzcai@scu.edu.cn; jbzhu@scu.edu.cn
First published on 6th January 2023
The development of inexpensive and high-performance chemically recyclable polymers serves as a promising strategy for solving the issues regarding plastic pollution. In the current work, we prepared a series of aromatic monomers (DHB-R and DHN-R, R = Me, Et) derived from aromatic hydroxy acids and epoxides. Ring-opening polymerization of these monomers afforded the semiaromatic polyesters P(DHB-R) and P(DHN-R) (R = Me, Et) with high molecular weights and narrow dispersity. Remarkably, these polymers showed high thermal stability with 335 °C < Td < 350 °C. Changing the benzene ring to a naphthalene ring on the polymer backbone led to a significant improvement in the glass transition temperature (Tg), from 49 to 100 °C. P(DHB-Me) behaved as a brittle and strong material, whereas P(DHB-Et) displayed excellent ductility with an elongation at break of 762.63 ± 94.40%. More importantly, P(DHB-R) and P(DHN-R) could be effectively and selectively depolymerized into the corresponding monomers, establishing a circular plastics economy.
In 2016, Shaver and co-workers reported the ROP of 2,3-dihydro-5H-1,4-benzodioxepin (DHB) to synthesize the analogues of PET (PDHB), which could be successfully recycled to the monomer DHB in dilute solution with the catalyst salen-Al (Fig. 1).60,61 However, the low thermal stability of PDHB (Td ∼ 180 °C) limited its further application. In a following work, Makwana, Lizundia and co-workers investigated the substituent effect on the meta-position of benzene ring, and revealed a resulting P(R-DHB) showing an improved thermal stability, specifically with a Td in the range of 230 to 260 °C.62 In 2021, the Li research group designed three constitutional isomers of benzo-thia-caprolactones with great chemical recyclability to monomers under bulk thermal conditions.63 The resulting semiaromatic polyesters displayed Td values ranging from 180 to 280 °C. In the meantime, our laboratory developed a facile one-pot synthetic method for preparing a library of benzo-thia-caprolactones with various substituents from thiosalicylic acid and epoxides as the reactants.64 The thermal and mechanical properties of the resulting aromatic polyesters could be tailored by subjecting them to functionalization and stereocomplexation to achieve high thermal stability (285 °C < Td < 310 °C) and polyolefin-like tensile performance.
Fig. 1 Representative examples of semiaromatic monomers based on 2,3-dihydro-5H-1,4-benzodioxepin (DHB). |
To further develop the PDHB system to meet practical applications as chemically recyclable polymers, we aimed to enhance its thermal and mechanical properties by leveraging the monomer structure. Motivated by our previous monomer design strategy based on epoxides,64–66 we were able to take advantage of the inexpensive and bio-derived salicylic acid and epoxides to synthesize DHB-Me and DHB-Et using a convenient two-step method. Furthermore, 3-substituted 2,3-dihydro-5H-naphthodioxepin-5-ones (DHN-R, R = Me, Et) were also prepared from 3-hydroxy-2-naphthoic acid and epoxides (Fig. 1). To our delight, these functionalized DHB/DHN-based monomers underwent efficient ROP and produced semiaromatic polyesters with excellent thermal stability (Td > 335 °C) and tunable thermal and mechanical properties, while maintaining chemical recyclability.
As 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) has been reported to be an effective organocatalyst for ROP of cyclic esters,67–76 TBD-catalyzed ROP of monomers was first investigated in bulk conditions. The polymerization of DHB-Me with a [DHB-Me]:[TBD]:[I] ratio of 100:1:1 reached 71% conversion within 1 h at 70 °C (Table 1, entry 1). As a comparison, DHB-Et with a bulkier ethyl substituent exhibited lower reactivity, approaching 69% conversion in 3 h under similar conditions (Table 1, entry 9). At an increased [monomer]:[TBD]:[I] ratio of 500:1:1, the polymerizations occurred with 76% and 60% conversions of, respectively, DHB-Me and DHB-Et in 12 h (Table 1, entries 2 and 10). The number-average molecular weights (Mns) of the resulting polymers were much lower than the calculated values (Mn, theos), indicating that this TBD catalytic polymerization system was not well controlled.
Entry | Monomer | Cat. | [M]/[I]/[Cat.] | Time/h | Conv.b/% | M n, theo /kDa | M n, SEC /kDa | Đ | T g /°C | T d /°C |
---|---|---|---|---|---|---|---|---|---|---|
a The polymerizations of DHB-Me and DHB-Et were conducted at bulk conditions, 70 °C; and the polymerizations of DHN-Me and DHN-Et were carried out in toluene solution (2 M) at 100 °C. b Calculated from the 1H NMR spectrum in CDCl3. c M n, theo = MW (monomer) × [M]0/[I]0 × Conv. + MW (terminal group). d Number-average molecular weight (Mn) and dispersity index (Đ = Mw/Mn) determined from the results of size exclusion chromatography (SEC) performed at 40 °C in THF. e T g measured from the results of differential scanning calorimetry (DSC), specifically from the second heating-scan curves with a cooling and second heating rate of 10 °C min−1. f T d measured from the results of thermal gravimetric analysis (TGA) carried out at a heating rate of 10 °C min−1. | ||||||||||
1 | DHB-Me | TBD | 100:1:1 | 1 | 71 | 12.6 | 9.1 | 1.22 | — | — |
2 | DHB-Me | TBD | 500:1:1 | 12 | 76 | 67.7 | 35.0 | 1.25 | 64 | 340 |
3 | DHB-Me | Zn1 | 500:1:1 | 2 | 64 | 57.0 | 45.0 | 1.34 | 65 | 342 |
4 | DHB-Me | Zn1 | 1000:1:1 | 6 | 75 | 134 | 97.6 | 1.19 | 65 | 343 |
5 | (R)-DHB-Me | TBD | 100:1:1 | 1 | 77 | 13.7 | 10.7 | 1.20 | 60 | 336 |
6 | (R)-DHB-Me | Zn1 | 500:1:1 | 6 | 60 | 53.4 | 36.6 | 1.25 | 63 | 345 |
7 | (S)-DHB-Me | TBD | 100:1:1 | 1 | 77 | 13.7 | 10.6 | 1.17 | 58 | 335 |
8 | (S)-DHB-Me | TBD | 500:1:1 | 6 | 63 | 56.1 | 36.6 | 1.23 | — | — |
9 | DHB-Et | TBD | 100:1:1 | 3 | 69 | 13.2 | 12.4 | 1.20 | — | — |
10 | DHB-Et | TBD | 500:1:1 | 12 | 60 | 57.6 | 31.1 | 1.24 | 48 | 342 |
11 | DHB-Et | Zn1 | 500:1:1 | 1 | 64 | 61.5 | 73.9 | 1.23 | 49 | 349 |
12 | DHB-Et | Zn1 | 1000:1:1 | 4 | 68 | 130 | 123 | 1.17 | 50 | 339 |
13 | DHN-Me | Zn1 | 100:1:1 | 1 | 74 | 21.3 | 20.0 | 1.25 | — | — |
14 | DHN-Me | Zn1 | 500:1:1 | 6 | 66 | 75.3 | 66.0 | 1.13 | 118 | 336 |
15 | DHN-Me | Zn1 | 1000:1:1 | 7 | 64 | 146 | 88.7 | 1.18 | 114 | 345 |
16 | (R)-DHN-Me | Zn1 | 100:1:1 | 1 | 74 | 16.9 | 14.9 | 1.38 | 109 | - |
17 | (R)-DHN-Me | Zn1 | 500:1:1 | 4 | 91 | 104 | 42.5 | 1.57 | 121 | 349 |
18 | (S)-DHN-Me | Zn1 | 100:1:1 | 1 | 71 | 16.2 | 13.1 | 1.39 | 110 | — |
19 | DHN-Et | Zn1 | 100:1:1 | 1 | 55 | 13.3 | 15.9 | 1.23 | — | — |
20 | DHN-Et | Zn1 | 500:1:1 | 3 | 54 | 65.4 | 44.6 | 1.13 | 100 | 344 |
21 | DHN-Et | Zn1 | 1000:1:1 | 6 | 52 | 126 | 66.7 | 1.10 | — | — |
To improve the polymerization efficiency of this system, the organometallic complex Zn177 was investigated as the catalyst. Gratifyingly, Zn1 displayed improved activity for the ROPs of DHB-Me and DHB-Et with turnover frequencies (TOFs) ranging from 125 to 320 h−1 (Table 1, entries 3, 4, 11 and 12). Impressively, P(DHB-Et) with a high Mn of 123 kDa and relatively narrow dispersity of 1.17 was obtained when using a [DHB-Et]:[Zn1]:[I] ratio of 1000:1:1 (Table 1, entry 12). The ROPs of DHN-Me and DHN-Et were carried out with Zn1 as a catalyst and p-tolylmethanol as an initiator in toluene at 100 °C, due to their high melting temperatures and poor solubility levels. Monomer conversions of 64% and 52% were achieved for DHN-Me and DHN-Et at a [monomer]:[Zn1]:[I] ratio of 1000:1:1, demonstrating TOFs of 91.4 h−1 and 86.7 h−1, respectively. The produced P(DHN-Me) and P(DHN-Et) showed a range of Mns from 15.9 to 88.7 kDa and a relatively narrow distribution of molecular weights (Đ < 1.25). Additionally, enantiopure monomers (R)-DHB-Me and (R)-DHN-Me underwent polymerization in a similar fashion as did racemic monomers and afforded isotactic P[(R)-DHB-Me] and P[(R)-DHN-Me] with Mns of 36.6 and 42.5 kg mol−1, respectively (Table 1, entries 6 and 17). Their isotactic arrangements were confirmed using 13C NMR spectroscopy, with the observation of only one set of resonances (Fig. S19 and S27†).
The linear structure and high fidelity of p-methylbenzyl terminal groups of the produced polymer were evaluated using matrix-assisted laser desorption ionization time-of-flight (MALDI-TOF) mass spectrometry (Fig. S34†). The MALDI-TOF mass spectrum of a P(DHB-Me) sample prepared from a 50:1:1 ratio of [DHB-Me]:[Zn1]:[I] displayed a series of molecular ion peaks showing a neighboring spacing of 178.38, which was consistent with the molar mass of the DHB-Me repeat unit. The intercept of a line fitted to the data was found to be 145.17, matching the total mass of chain ends plus the mass of Na+ [Mend = 122.17 (CH3C6H4CH2OH) g mol−1 + 23 (Na+) g mol−1], confirming the linear structure of CH3C6H4CH2O–[DHB-Me]n–H.
Thermal gravimetric analysis (TGA) and differential scanning calorimetry (DSC) were utilized to assess the thermal properties of the produced polymers. All these polymers exhibited excellent thermal stability—with the onset decomposition temperature (Td), defined as the temperature at 5% weight loss, ranging from 336 °C to 349 °C (Fig. 2a). These values were about 160 °C higher than that of P(DHB),61 highlighting the significant improvement in thermal stability resulting from including the substitutions in P(DHB).
Fig. 2 Thermal properties of the produced semiaromatic polyesters. (a) TGA curves of P(DHB-Me), P(DHB-Et), P(DHN-Me), and P(DHN-Et). (b) DSC curves of P(DHB-Me), P(DHB-Et), P(DHN-Me), and P(DHN-Et). |
P(DHB-Me) and P(DHB-Et) showed glass transition temperature (Tg) values of 65 °C and 49 °C, respectively. In contrast, P(DHN-Me) and P(DHN-Et) showed higher Tg values of 118 °C and 100 °C (Fig. 2b), which could be attributed to the more rigid naphthalene structures in these two polymers. The absence of a melting transition revealed the amorphous feature of these polymers. Initially, we hypothesized that the lack of crystallinity was due to their atactic structures. The thermal transitions of isotactic P[(R)-DHB-Me] and P[(R)-DHB-Me] were subsequently investigated. Surprisingly, melting transitions were observed neither for P[(R)-DHB-Me] nor for P[(R)-DHN-Me] (Fig. S43 and S46†). Compared with the previously reported sulfur-containing systems,64 we inferred that the heteroatoms in the system might be responsible for the crystallinity of the material. We investigated the stereocomplexation of the polymers by mixing isotactic (R)-polymer and (S)-polymer in a 1:1 molar ratio (approximately 100 mg in total). Unfortunately, no stereocomplexation was observed for either of these systems. DSC and PXRD analyses were carried out to characterize the formation of stereocomplexes (Fig. S56†). However, melting transitions were neither observed for the isotactic polymers nor for their blends. Additionally, the absence of sharp peaks for (R)-polymer, (S)-polymer, and their mixture in their PXRD patterns further confirmed the amorphous character of the polymers.
The enhanced thermal properties of these semiaromatic polyesters encouraged us to investigate their mechanical properties. Uniaxial tensile tests were performed on hot-pressed dogbone-shape films at an extension rate of 10 mm min−1 (Fig. 3). P(DHB-Me) behaved as a stiff material with high tensile strength (σB = 33.69 ± 5.39 MPa), Young's modulus (E = 2.17 ± 0.36 GPa), and elongation at break (εB = 10.91 ± 2.15%). In comparison to P(DHB-Me), the isotactic P[(R)-DHB-Me] and P[(S)-DHB-Me] displayed similar tensile performances (Table S4 and Fig. S58†). In contrast, P(DHB-Et) displayed a σB value of 3.16 ± 0.57 MPa and an εB of 762.63 ± 94.40%. The distinct tensile performances of P(DHB-Me) and P(DHB-Et) manifested the profound impact of pendant groups on the mechanical properties of polymers. We hypothesized that the ethyl substituents in P(DHB-Et) were more flexible than the methyl side chain in P(DHB-Me), and that this difference in flexibility contributed to a significant difference between the packings of the polymer chains. Moreover, the Tg value of P(DHB-Et) was close to room temperature, which also led to the improved ductility of the P(DHB-Et) film measured at room temperature. P(DHN-Me) and P(DHN-Et) appeared to be brittle with an εB < 5% and σB > 35 MPa. We believe that the strength and brittleness of these polymers were due to the rigidity of their naphthalene moieties. Interestingly, attempts to improve the ductility of P(DHB-Me) via copolymerization with DHB-Et was unsuccessful. A copolymer P(DHB-Me-Co-DHB-Et) with only 7 mol% DHB-Me was prepared by carrying out a one-pot copolymerization of DHB-Me and DHB-Et in a [DHB-Me]:[DHB-Et]:[Zn1]:[I] feed ratio of 50:1000:1:1 (with the composition determined from 1H NMR analysis, Fig. S32†). This P(DHB-Me-co-DHB-Et) copolymer (Mn = 57.5 kDa, Đ = 1.13) performed as a hard and tough material like P(DHB-Me) with σB = 38.16 ± 3.56 MPa and εB = 5.86 ± 0.65%.
Fig. 3 (a) Images of the polymer films used for the tensile test. (b) Stress–strain curves of the produced polymers. |
Prior to performing the chemical recycling study, we investigated the thermodynamics of the ROP of DHB-Me at [DHB-Me]0 = 2 M (Fig. S63†). The thermodynamic parameters and were calculated to be −14.8 kJ mol−1 and −43.3 J mol−1 K−1, respectively. The ceiling temperature Tc at an initial monomer concentration of 1 mol L−1 was determined to be 69 °C according to the equation , indicative of excellent recyclability. Chemical recycling to monomers of these synthesized polymers were next tested in dilute solution. With 5 mol% Zn1 loading, the depolymerizations of P(DHB-Me) and P(DHB-Et) underwent nearly quantitative conversions to DHB-Me and DHB-Et in 30 minutes at 120 °C (Fig. 4 and Fig. S64†), while P(DHN-Me) and P(DHN-Et) showed moderately lower yields of 80% and 83% at 140 °C (Fig. S65 and S66†). When 10 mol% TBD was used as a catalyst, DHN-Me and DHN-Et were selectively recycled with high conversions of 93% and 98%, respectively (Table S10†). These results demonstrated a high efficiency for the chemical recycling of these synthesized polymers.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2py01491b |