C. Yeonab,
G. Kimab,
J. W. Limab and
S. J. Yun*ab
aICT Materials & Components & Research Laboratory, Electronics and Telecommunications Research Institute, 218 Gajeongno, Yuseong-gu, Daejeon 305-700, Korea. E-mail: sjyun@etri.re.kr
bDepartment of Advanced Device Engineering, University of Science and Technology, 217 Gajeongno, Yuseong-gu, Daejeon 305-350, Korea
First published on 20th October 2016
In this study, the conductivity of poly(3,4-ethylenedioxythiophene):poly(4-styrenesulfonate) (PEDOT:PSS) was greatly enhanced by using sodium dodecyl sulfate (SDS) without damaging the fabric substrates. We suggest that blending and dipping methods using SDS which is compatible with natural and synthetic fabrics dramatically increase the conductivity of PEDOT:PSS to as high as 1335 S cm−1. Additionally, a highly stretchable fabric heater with high conductivity was successfully fabricated using SDS-modified PEDOT:PSS. The fabric heaters exhibited reversible electrical behaviour with cyclic loading of a tensile strain even larger than 80%. The increase in resistance with the tensile strain was significantly smaller than the calculated value for a rigid substrate because the fabrics with a weave structure exhibited interfibrillar contact effects with strain. For example, the resistance was increased by a factor of only 2.62 with 80% strain. The Joule heating behaviours of the fabric heaters were demonstrated at several different applied voltages and ambient temperatures, and the heat capacity and convective heat transfer coefficient were 2 J K−1 and 30 W m−2 K−1, respectively. The results demonstrated that the method suggested in this work is not only efficient for greatly improving the conductivity but also simple and cost-effective for fabricating highly conductive and stretchable fabrics with various e-textile applications.
The conductivity of PEDOT:PSS has been reported to be increased by the addition of dielectric organic solvents, such as dimethyl sulfoxide (DMSO),23 or by post-treatment with a strong acid.24 However, the use of DMSO may irritate human skin, and fabrics are vulnerable to acid, preventing the use of post-treatment with a strong acid. Therefore, to improve the performance of PEDOT:PSS for application in the development of wearable heaters, it will be necessary to increase the conductivity of PEDOT:PSS without causing damage to the fabric.
Sodium dodecyl sulfate (SDS), one of the ionic surfactants that have been generally used in detergents for laundry, is effective for increasing the conductivity of PEDOT:PSS. It was reported that the conductivity of PEDOT:PSS film can be increased to 80 S cm−1 by adding SDS into PEDOT:PSS aqueous solution (hereafter, simply denoted by blending method).25 However, previous study on the effect of anionic surfactants in PEDOT:PSS have not been studied in detail for achieving high conductivity.
In this study, we report the most effective and simple process using SDS for fabrication of highly conductive PEDOT:PSS, and SDS-modified PEDOT:PSS was evaluated as a conductive material in fabric heaters. The Joule heating properties of the stretchable fabric heater was also described.
The Joule heating behaviours of fabric heaters were investigated under constant voltages (6, 9, and 12 V) supplied by a DC power source (RDP-305; SMART). We measured the temperatures of the heaters using a digital thermometer (UT320; UNI-T) and observed their IR images using a thermal camera (Therm-App TH, Therm-App). The resistances of the fabric heaters with or without strain were obtained from I–V characteristic curves of the samples using a source meter (4200-SCS; Keithley). The joule heating experiment was carried out at an ambient temperature of 26 °C. The experiment at 4 °C was also carried out in a refrigerator to show the heating behaviour in a cold environment.
We suggested two methods for applying SDS to PEDOT:PSS for applications involving fabrics: the blending method, in which fabrics are impregnated with a PEDOT:PSS aqueous solution blended with SDS; and the dipping method, in which fabrics are dipped in an aqueous solution containing PEDOT:PSS and SDS. In order to develop the most effective process for achieving high electrical conductivity and mechanical stability for applications as wearable heaters, the effects of SDS blending and dipping methods were evaluated by varying the SDS concentration.
A glass substrate was used for the electrical characterization of PEDOT:PSS films formed by blending and dipping methods. The conductivity and thickness of the films formed by the blending method (denoted as B-PEDOT:PSS films) are plotted with respect to the SDS concentration in the blended solution in Fig. 1a. The conductivity of the PEDOT:PSS film logarithmically increased as the SDS concentration was increased from 0 to 40 mM, and the highest conductivity of 465 S cm−1 was achieved at 40 mM SDS. The film thickness also increased gradually from 80 to 110 nm with as the SDS concentration increased. A non-uniform film was obtained at concentrations above 40 mM, owing to aggregation during spin-coating. The conductivity and thickness of the films formed by the dipping method (denoted as D-PEDOT:PSS films) are shown in Fig. 1b. The conductivity was significantly increased from 0.5 to 1008 S cm−1 with increasing concentrations of SDS solution from 0 to 400 mM. Additionally, the film thickness decreased from 80 to 30 nm with increasing concentrations of SDS aqueous solution, similar to the behaviour of PEDOT:PSS films treated with a strong acid, such as H2SO4, HNO3, or HCl.26,27 Thus, these results suggested that the mechanism of conductivity enhancement in PEDOT:PSS for blending and dipping methods is quite different.
The stability test was performed under constant conditions (relative humidity and temperature were 40% and 22.5 °C, respectively) for 7 days. As shown in Fig. 1c, the conductivities of B-PEDOT:PSS and D-PEDOT:PSS films remained almost unchanged, while the pristine PEDOT:PSS film underwent severe degradation. The normalised conductivity (σ/σ0) with respect to time is shown in the inset in Fig. 1c, where the value of σ/σ0 at a time represents the ratio of the initial conductivity (σ0) and the conductivity measured after the time (σ). The σ/σ0 of the pristine PEDOT:PSS film decreased to 0.5 within 1 day. In contrast, the σ/σ0 values of B-PEDOT:PSS and D-PEDOT:PSS films were 0.96 and 0.95, respectively, after 7 days.
To investigate the mechanism of conductivity enhancement through the blending and dipping methods, the analysis of chemical bonding states of PEDOT:PSS films was carried out using absorption spectroscopy. The absorption spectra of the PEDOT:PSS films formed by SDS blending (40 mM) and SDS dipping (40, 100, 200, and 400 mM) are shown in Fig. 2a. Notably, the D-PEDOT:PSS films showed significant decreases in absorbance at 5.5 eV, where a strong absorption band originated from the aromatic rings of PSS.28 This result demonstrated that insulating PSS in the film was selectively removed. A small increase in absorbance in the region from 1 to 2 eV was also observed, indicating the generation of polaronic states in the bandgap due to enhancement of the interchain interaction between the conducting domains.29 In contrast, for the B-PEDOT:PSS film, absorbance in the UV light region increased due to absorption by SDS, with no increase in absorbance in the region from 1 to 2 eV (ESI Fig. S2†).
Raman spectroscopic analysis was also carried out to investigate conformational changes in the pristine and SDS-modified PEDOT:PSS films. As shown in Fig. 2b, the Raman spectra showed two intensive peaks, which could be attributed as follows: 1438 cm−1 to Cα–Cβ symmetric stretching vibrations, 1373 cm−1 to Cβ–Cβ deformations.30 The Raman spectrum of the B-PEDOT:PSS film showed an 8 cm−1-shifted Cα–Cβ symmetric stretching vibrational peak to a higher energy compared with that of pristine PEDOT:PSS. The degree of blue shift of the Cα–Cβ symmetric stretching peak gradually increased with the concentration of SDS (ESI Fig. S3†). These results suggested that the SDS introduced into PEDOT:PSS solution can replace PSS as the counter-anions to PEDOT chain resulting in conformational change from benzoid (coiled) to quinoid (linear) structure.25,31 Contrary to pristine- and B-PEDOT:PSS films, the Cα–Cβ symmetric stretching peak of the D-PEDOT:PSS film was red-shifted. Although this red-shift implied that the conformation of PEDOT:PSS was changed from quinoid to benzoid structure, conductivity of D-PEDOT:PSS dramatically increased because the PEDOT oxidation state changes from bipolaron to polaron by the PSS removal as supported by the increase of polaronic states in absorption spectra of Fig. 2a.
The conformational change of PEDOT:PSS could also affect the bonding energy between constituent atoms in PEDOT:PSS.32 Thus, FT-IR analysis was performed to investigate the change of bonding energy. As shown in Fig. 2c, the FT-IR spectrum of the pristine PEDOT:PSS showed peaks at 1209, 1143, and 1089 cm−1 which are originated from to C–O–C bond stretching in the ethylene dioxy group.33,34 The C–S bond stretching peaks in the thiophene ring were observed at 977, 827, and 690 cm−1.33,34 The peaks assigned at 1544 and 1342 cm−1 correspond to CC and C–C bonds, respectively.33,34 These peaks in the FT-IR spectrum of D-PEDOT:PSS shifted to higher bonding energies, while the FT-IR spectrum of B-PEDOT:PSS was similar to that of pristine-PEDOT:PSS. In particular, the peak of 1342 cm−1 corresponding to the C–C bond shifted to 1432 cm−1, which means that the C–C bonding energy increased due to the PSS removal by SDS dipping.
Based on the results, schematic conformations of the pristine-, B-, and D-PEDOT:PSS were illustrated in Fig. 2d. The SDS blending method induces the conformational change from coiled to linear structure by introducing SDS molecules and the SDS dipping method selectively removes PSS domains to increase the interchain interactions between PEDOT-rich cores.
Distinct changes in the surface morphologies of B- and D-PEDOT:PSS films were observed by atomic force microscopy (AFM). The AFM images of topography in Fig. 3a, c and e demonstrate that the rms roughness (Rq) values of the pristine- and B-PEDOT:PSS films were 1.3 and 1.4 nm, respectively, and the Rq of D-PEDOT:PSS films increased to 2.2 nm. Fig. 3b, d and f show phase images in which the positively charged (bright) and negatively charged (dark) phases corresponded to PEDOT-rich and PSS-rich grains, respectively.35 These results clearly supported that the SDS dipping method induced selective removal of PSS domains. In contrast, the phase image of B-PEDOT:PSS (Fig. 3d) was similar to the image of pristine-PEDOT:PSS (Fig. 3b), indicating that the conductivity enhancement conferred by the SDS blending method was caused not by PSS removal but by conformational change of PEDOT chains.
Next, we found that application of the blending method followed by the dipping method could further increase the conductivity. As shown in Fig. 4a, the highest conductivity of 1335 S cm−1 could be achieved by using both the blending and dipping methods. The same trend was obtained in the case of the fabric impregnated with PEDOT:PSS (ESI Fig. S4†).
Fig. 4 (a) The highest conductivities of B-, D-, and BD-PEDOT:PSS films spin-coated on glass. (b) Sheet resistance (RS) and weight of PEDOT:PSS of BD-PEDOT:PSS-cotton and polyurethane. |
Fabrics can be easily impregnated with aqueous PEDOT:PSS solution as long as the fabrics can be wetted by water. In this study, 100% polyurethane (denoted as polyurethane) and 98% cotton/2% polyurethane (denoted as cotton), which exhibited high stretchability, were used for the fabrication of conductive and stretchable fabric (ESI Fig. S5†). Hereafter, the fabrics impregnated in SDS-blended PEDOT:PSS solution followed by dipping SDS aqueous solution are denoted as BD-PEDOT:PSS-fabrics. As shown in Fig. 4b, the sheet resistances (RS) for BD-PEDOT:PSS-cotton and -polyurethane were 24 and 48 Ω □−1, respectively. The results indicated that the RS of the BD-PEDOT:PSS-cotton was lower than that of the BD-PEDOT:PSS-polyurethane because the amount (1.6 mg cm−2) of PEDOT:PSS coated on the cotton was higher than that (0.7 mg cm−2) coated on the polyurethane. Furthermore, the RS value could be gradually decreased by increasing the number of coatings (ESI Fig. S6†). Depending on the porosity and hydrophilicity of fabrics, the RS of BD-PEDOT:PSS-fabric could be further decreased, and the style of weave that could absorb large amounts of PEDOT:PSS was important for achieving a low RS value.
In order to investigate the stretchability of the PEDOT:PSS-modified fabrics and to determine which fabric would be most valuable for conferring conductivity, the resistance was measured under tensile strain (ε). The initial resistance of a sample before loading any strain, R0, is described by eqn (1),
(1) |
(2) |
(3) |
The woven structure of the fabric related to the Poisson's ratio determines its structural and mechanical properties.38 Thus, the νs values of cotton and polyurethane used as fabric substrates in this work were measured to be 0.48 and 0.2, respectively. The reported νf of PEDOT:PSS was 0.3532. As shown in Fig. 5a, we plotted RSt/R0 with respect to ε for BD-PEDOT:PSS-cotton (solid line), where the resistances were directly measured from the current (I)–voltage (V) characteristic curves of the samples. The method of I–V measurement is described in detail in Fig. S7.† The RSt/R0 values calculated using the νs and νf mentioned above are shown in Fig. 5a (dotted line). The measured RSt/R0 values with ε ≤ 20% were consistent with the calculated values, and the differences between them increased with ε when ε > 20%. For example, at ε = 80%, the measured RSt/R0 of the BD-PEDOT:PSS-cotton was 2.62, while the calculated RSt/R0 was 4.05. The significantly small increase in the real RSt with ε compared with the calculated value must be caused by the woven structure of the fabric. The stretching of the fabric improves the alignment and intercontact of the fibres, thereby reducing its resistance.39,40 Hereafter, we call this effect the “interfibrillar contact effect”.
Next, the cyclic ε-loading/unloading tests were performed for BD-PEDOT:PSS-cotton was also performed and the result was shown in Fig. 5b. The RSt/R0 shows reversible behaviour with cyclic ε-loading/unloading. The inset in Fig. 5b shows the changes in RSt/R0 during a cycle of ε-loading/unloading. The difference of RSt/R0 between ε = 0% (blue arrow) and 20% (red arrow) was only 0.09. However, the difference gradually decreased with the strain, and finally showed reaching a negative value. For example, the difference was decreased from 0.09 to −0.20 when the strain increased from 20% to 80%. The results clearly indicated that the interfibrillar contact effect increased with ε due to the increase of in the interfibrillar contact area along with the axis of ε until the cotton was torn at ε > 80%.
We also carried out I–V measurement and cyclic ε-loading/unloading tests for BD-PEDOT:PSS-polyurethane, which was stretchable even with an extreme strain greater than 150%. The calculated and experimental RSt/R0 curves for BD-PEDOT:PSS-polyurethane are shown in Fig. 5c. The measured RSt/R0 values with ε = 40% coincided with the calculated values, and the difference between them then increased with ε when ε > 40%. The results of cyclic ε-loading/unloading tests for BD-PEDOT:PSS-polyurethane are shown in Fig. 5d. Interestingly, the RSt/R0 values of BD-PEDOT:PSS-polyurethane were saturated after only a few cycles of ε-loading/unloading, even with an ε value as large as 80%, and the results consistently showed reproducible curves by ε-loading/unloading. The inset of Fig. 5d clearly demonstrates that the interfibrillar contact effect was still effective with ε = 150%.
In this work, we introduce the term “critical interfibrillar contact strain (εCIC)”, above which the experimental RSt/R0 values begin to deviate from the values calculated using Poisson's ratios; when ε > εCIC, (RSt/R0)exp < (RSt/R0)cal for a positive interfibrillar contact effect. As shown in Fig. 5a and c, the εCIC of BD-PEDOT:PSS-polyurethane (νs = 0.2) was 40%, while the εCIC of BD-PEDOT:PSS-cotton (νs = 0.48) was 20%. These results implied that the value of νs was related to εCIC and that larger νs values resulted in smaller εCIC values. Moreover, higher νs values could more effectively facilitate increased interfibrillar contact effects during stretching.
As shown in Fig. 5b and d, the relaxed resistance, R′0, even after one cycle of ε-loading/unloading, was larger than R0, and RSt/R0 was not recovered to the initial value of 1.0. This may be explained by the permanent deformation of the conducting films owing to cracking or peeling. To investigate the reason for this deformation, we used optical microscopy and scanning electron microscopy (SEM) before and after ε-loading for the BD-PEDOT:PSS-cotton, which was relatively weak against strain compared with BD-PEDOT:PSS-polyurethane. Fig. 6a shows optical and SEM images of the BD-PEDOT:PSS-cotton before and after ε-loading. These optical images showed that the BD-PEDOT:PSS-cotton (purple colour) was uniformly coated by PEDOT:PSS. The SEM image in Fig. 6b does not show any visible fractures after loading 40% of ε. However, the PEDOT:PSS films showed signs of peeling at ε = 150% (ESI Fig. S8†). In a previous study, a compressive force perpendicular to the stretching direction was exerted on the film during stretching, leading to the formation of cracks when the Poisson's ratio of the substrate was larger than that of the film,36 and we observed cracks in SDS-modified PEDOT:PSS coated on polydimethylsiloxane, even after loading 40% of ε (ESI Fig. S9†). These results demonstrated that the woven structure significantly relieved stress from the compressive force; therefore, BD-PEDOT:PSS-fabric exhibited excellent stretchability while maintaining low resistance. This low resistance behaviour with a very large ε may be a noticeable advantage of conductive fabric applications compared with conventional plastic applications.
Fig. 6 Optical and SEM images of the BD-PEDOT:PSS-cotton before (a) and after (b) loading 40% tensile strain. The scale bar of the SEM image is 10 μm. |
Using the BD-PEDOT:PSS-cotton, we fabricated a flexible heater to determine the applications of stretchable conducting fabrics and evaluated the Joule heating behaviours of this heater. Fig. 7a shows the temperature (T)–time (t) profiles for the BD-PEDOT:PSS-cotton, which had an RS of 24 Ω □−1. When a bias voltage (6, 9, or 12 V) was applied, the temperature of the fabric heater increased and saturated to a certain temperature within 60 s. For example, the saturated temperature (Tsat) of BD-PEDOT:PSS-cotton was 99.6 °C when 12 V was applied. The heat capacity (C) and convective heat transfer coefficient (h) could be also obtained by comparing the experimental data with the T–t curve calculated using a power balance equation.41
In general, a power balance equation41 between the input power and heat loss by convection (Qconv) and radiation (Qrad) can be described as shown in eqn (4),
(4) |
Qconv = hA(T − T0) | (5) |
Qrad = eσA(T4 − T04) | (6) |
(7) |
To evaluate the potential of stretchable PEDOT:PSS-fabric heaters, the Joule heating behaviours were investigated with different ε values. As shown in Fig. 7b, the value of Tsat decreased slightly from 99.6 to 97.7 °C at ε = 10%. Additionally, the Tsat was 80.4 °C at ε = 80%. The values of Tsat with respect to ε were plotted in Fig. S10.† As inferred from Fig. 5a, the experimental values of Tsat with ε > 20% were larger than the calculated values due to the interfibrillar effect. These results indicated that the BD-PEDOT:PSS-fabric was a promising material for application in highly stretchable heaters.
In practical applications, fabric heaters may be used in a cold environment. Therefore, the heating behaviours were also investigated in a low-temperature environment (4 °C) and compared with the heating behaviours at room temperature (26 °C). As shown in Fig. 7c, the Tsat of BD-PEDOT:PSS-cotton was 88.0 °C, while the value at room temperature was 99.6 °C. Furthermore, a longer time was needed to reach saturation at 4 °C than at 26 °C. This result could be explained by changes in h depending on environmental conditions (the speed of convection currents, etc.).42
We also obtained photographs and infrared images of a human hand wearing the fabric heater, as shown in Fig. 7d. In this experiment, the input voltage was as mild as 6 V to avoid the potential danger of burns. The maximum (Tmax) and minimum temperatures (Tmin) were 46.1 and 41.9 °C, respectively, before bending the finger, and 46.9 and 42.6 °C, respectively, after bending the finger. The results clearly show that BD-PEDOT:PSS-fabric can be adaptable even for the finger joint or elbow requiring very high stretchability (ε > 100%).
As described above, because a few cycles are needed to reach a stable reversible behaviour, a cycle-aging process at a certain ε is essential for practical applications requiring consistent reproducible performance. Fig. 8 shows the RSt/R0,sat′ values of BD-PEDOT:PSS-fabrics during a cycle of 80% ε-loading/unloading, where R0,sat′ is the saturated resistance of a sample at ε = 0% after suffering from cycle-aging processing at ε = 80%. The results showed that the differences between the maximum and minimum RSt/R0,sat′ values for BD-PEDOT:PSS-cotton and polyurethane were 0.09 and 0.11, respectively; these values are so small that stretchable device performance would not be noticeably changed with respect to variations in ε during practical operation.
Fig. 8 The RSt/R0,sat′ values of (a) BD-PEDOT:PSS-cotton and (b) BD-PEDOT:PSS-polyurethane during a cycle of 80% loading after performing the cycle-aging process at ε = 80%. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra24749k |