Naidu Dhanpal Jayrama,
S. Soniaa,
Palaniswamy Suresh Kumarb,
L. Marimuthua,
Yoshitake Masudac,
D. Mangalaraj*a,
N. Ponpandiana,
C. Viswanathana and
Seeram Ramakrishnad
aDepartment of Nanoscience and Technology, Bharathiar University, Coimbatore-641 046, India. E-mail: dmraj800@yahoo.com
bEnvironmental & Water Technology, Centre of Innovation, Ngee Ann Polytechnic, Singapore 599489, Singapore. E-mail: sureshinphy@yahoo.com
cNational Institute of Advanced Industrial Science and Technology (AIST), 2266-98 Anagahora, Shimoshidami, Moriyama-ku, Nagoya 463-8560, Japan
dCenter for Nanofibers and Nanotechnology, Department of Mechanical Engineering, National University of Singapore, Singapore 117576
First published on 15th May 2015
Highly monodispersed Ag embedded SiO2 nanostructured thin films are synthesized and their sensitivity towards SERS investigated. The possible mechanism for the formation of a highly monodispersed SiO2 nanostructured thin film and its self-assembled nanogap with Ag are discussed. It is found that the architecture of Ag embedded SiO2 (Ag@SiO2) are drastically influenced by precursor concentration and the reaction time. The morphology and monodispersity of the silica thin film were confirmed using FESEM and AFM. The crystallinity and existence of Ag on SiO2 were confirmed using XRD and XPS. The substrate shows enhanced SERS efficiency due to the reduced size (around 15 nm) of the Ag nanoparticles and the nano gap of (below 3 nm) between SiO2 and Ag. Based on the FDTD (finite-difference time-domain) simulation, the creation of hotspots was confirmed for the obtained nanogap. The prepared thin film possesses strong Surface Plasmon Resonance (SPR) with widely tunable peaks between 407–430 nm in the UV visible spectrum. The Ag@SiO2 nanosphere-based SERS platform provides highly enhanced effects and reveals a reproducible enhancement (EF = 7.79 × 108) of R6G (Rhodamine 6G), allowing a detection limit from a 10–18 mol L−1 solution. The prepared substrate was also used to detect trace levels of melamine from a 10–8 mol L−1 solution.
From the SAED pattern of TEM analysis we confirmed that the prepared nanoparticles are polycrystalline. The calculated lattice constant values a = b = c = 4.0344 Å are consistent with the standard JCPDS data. Fig. 3(a and b) shows the XPS spectrum of Ag embedded silica which confirms the presence of metallic silver. The Ag 3d core level signals can be well fitted with the two peaks at binding energy values of 373.7 eV and 367.7 eV, corresponding to the Ag 3d3/2 and Ag 3d5/2 signals respectively. The XPS data substantiate that Ag nanospheres are self-assembled on the Si surface by Ag–Si chemical bonds.28 Also, the doublet peaks located at 367.7 and 373.7 eV can be assigned to Ag (0) according to a previous report.29 These results indicate that the oxidation state of Si in the Ag@SiO2 nanospheres is well sustained during the vertical growth deposition. So the LSPR that occurred between them could be confirmed for SERS intensity.
Fig. 3 (a) XPS spectra of Ag (hydrosol A) embedded SiO2 nanospheres (b) corresponding magnified spectra of Ag. |
The prepared Ag and Ag@SiO2 nanostructured thin films were dispersed in ethanol and subjected to UV-Visible spectroscopy analysis. The reduction of Ag(I) to zero valent Ag nanoparticles was confirmed by the colour change of solution from colorless to yellow (Ag hydrosol A) and colorless to red (Ag hydrosol B)30 which correspond to absorption peaks at 429.24 and 407.28 nm respectively which are shown in Fig. 4. Ag nanoparticles exhibit surface plasmon resonances which are mostly sharp and well separated from interband transitions.
The red shift of the absorption wavelength and the broadening of the band for Ag hydrosol A are related to the larger particles. This is due to the dipole–dipole interaction among Ag nanoparticles deposited on the dielectric silica nanosphere and also electromagnetic coupling which enhances the polarizability of the electron cloud resulting in red shift of Surface Plasmon Resonance (SPR).31 The single and strong SPR bands indicate the formation of Ag nanoparticles through transverse and longitudinal resonances which are spherical in shape.32 The absorbance spectra of silica nanoparticles absorbed at 320 nm represent the specific peak for Si–O–Si bond which confirms the presence of silica nanoparticles. After the deposition of Ag nanoparticles onto the SiO2 spheres, broad and less intense peak appeared at 432.22 nm (SiO2 in Ag hydrosol A) and sharp and high intense peak appeared at 430.66 nm (SiO2 in Ag hydrosol B) due to the increase in the local refractive index of the surrounding medium for the Ag nanospheres caused by the formation of silica nanospheres and Mie Plasmon resonance excitation from the Ag nanoparticles.33 There is a slight red shift in absorption wavelength with increasing the size of the silver nanoparticles exhibiting stronger Plasmon resonance.34,35 The quantitative analysis of silver hydrosol A and B using SEM images Fig. 7(e and f) shows the size distribution of different silver nanoparticles. The normal curve function which show average size distribution of silver hydrosol A and B (see Fig. S3†). Thus in case of silver hydrosol B the increase in the intensity is due to participation of more no of particles for Surface Plasmon Resonance compare to silver hydrosol A. This elucidates a difference of 2 nm in the UV analysis for Ag@SiO2 A and B.
For the growth of silica, two main models have been emerged i.e. the ‘monomer addition model’ and the ‘aggregation growth model’. But still the debate is not over and new growth mechanisms have been postulated.36 Our findings conclude that growth occurs due to aggregation, where the primary particles with broad size distribution are generated in solution over a long time. The growth process of silica nanospheres were sequentially investigated using field emission scanning electron microscopy (see Fig. S2†).
Growth process of SiO2 nanospheres is shown in Fig. 5. Island like structures with a size of 1–2 μm were formed through a proper combination of constituents (60 mL ethanol, 0.78 mL TEOS, and NH3, 8 pH) which was constantly stirred for 5 min. An agglomeration of silica beads (150–200 nm) was formed under the same conditions with the addition of 5 mL of distilled water. On increasing the water concentration (10 mL) and pH (10), self-assembled arrays of silica nanospheres (Fig. 6(a–c)) were formed. So, the water molecules lead to faster kinetics and promote the nucleation of silica. In addition to this, the presence of ammonia promotes the formation of spherical particles. The effect of solvent and the presence of ammonia are the promising factors for the formation of highly ordered monodispersed spheres.37,38
Fig. 5 Growth mechanism of silver embedded silica nanospheres ((i) absence of H2O, (ii) 5 mL H2O, (iii) 10 mL H2O, (iv) 10 mL H2O + pH 10). |
Fig. 6 (a–c) FESEM micrographs of SiO2 with different magnifications (d) cross section image of SiO2 nanospheres. |
The proposed reaction mechanism is
Si–OR + H2O → Si–OH + ROH | (1) |
Si–OR + Si–OH → Si–O–Si + ROH | (2) |
In our experiment, the Ag nanoparticles were deposited using two hydrosols as described in the experimental session. Fig. 7(a and b) shows HR-TEM image and its SAED pattern where the hkl value for the plane (111), (222) confirms face centered cubic structure of Ag nanoparticles which well matches with XRD. Also the attachments of AgNPs with SiO2 nanospheres show a gap of less than 5 nm as shown in Fig. 7(c and d). These give strong evidence of hot spots for SERS studies.
Ag films prepared from both hydrosols show that the Ag nanoparticles are isolated from each other with no aggregation and it is clear that the size of Ag nanoparticles obtained using hydrosol A is bigger than those with Ag hydrosol B. As seen in Fig. 7(e and f) the Ag nanospheres obtained using Ag hydrosol A and B were in the size ranges of 15–20 nm and 5–10 nm respectively. The high degree of super saturation of NaBH4 leads to the formation of smaller silver nanoparticles. The positively charged silver nanoparticles prepared from hydrosol B cling onto the surface of silica nanospheres due to the negative surface charge of silica (see Fig. S4–S7†). As shown in Fig. 8(a–c), the negatively charged silver nanoparticles (hydrosol A) assemble in the nanogap between silica nanoparticles which may be due to the capillary forces41 and in the present case, the silica nanospheres array can act as the channel. The surface charge of Ag nanoparticles was confirmed by zeta potential analysis (see Fig. S8†) and the relationship between interparticle gap and SERS activity for Ag nanoparticle shows a dramatic enhancement when the size is in between 15–20 nm.42–46 As a result, Ag@SiO2 nanospheres obtained using Ag hydrosol A are considered as promising SERS substrates owing to their unique morphology. The atomic percentages of Si (35.21 at%), O (53.14 at%) and Ag (11.65 at%) confirm the formation of Ag@SiO2 nanospheres (Fig. 8(h)) and color mapping shows the elemental analysis of Ag@SiO2 (Fig. 8(d–g)). The red dots indicate the Ag peaks while the green and blue dots indicate the silicon dioxide.
Fig. 8 (a–c) FESEM micrographs of Ag@SiO2 thin films with different magnifications (d–g) color mapping image of Ag@SiO2 nanospheres (h) EDAX spectra of Ag@SiO2 [note: here Ag represents hydrosol A]. |
Roughness is one of the most important parameters for SERS. When the molecules are adsorbed to the metallic surfaces and exhibit atomic scale roughness, the Raman signal intensity is enhanced by 104 to 106 times. Fig. 9(a–e) represents the 2D and 3D images of SiO2 and Ag@SiO2 nanospheres which are identical with the FE-SEM images. Fig. 9(c and f) presents the two-dimensional histograms containing surface height values determined from the respective topographies. The obtained SiO2 and Ag@SiO2 nanospheres exhibited root-mean-square (RMS) roughness values of 14.9057 and 26.004 nm respectively and show high monodispersity of nanospheres.
Fig. 9 AFM 2D and 3D images of (a and b) SiO2 nanospheres (d and e) Ag@SiO2 nanospheres and (c & f) histograms of SiO2 and Ag@SiO2 nanospheres [note: here Ag represents hydrosol A]. |
The finite-difference time-domain (FDTD) method is adopted using lumerical solution-8. Intensity (|E|2) distributions are obtained from 3D FDTD calculations based on the following parameters: SiO2 (glass) palik material has been used as material, where the diameter of noble metal nanoparticles was 20 nm and an interparticle gap of 5 and 2.5 nm between silica and silver was chosen. Laser with 514 nm wavelength was employed. The detailed process is illustrated in Fig. 10. The maximum intensity (|E|2) of each noble metal/semiconductor was 112. As the SERS signals were proportional to the value of (|E|2), the 20 nm silver nanoparticles give larger SERS enhancement. Similarly in Fig. 10(a), when the gap between silica and silver is around 2.5 nm the hot spots increase and give strong electric field enhancement, while in the case of Fig. 10(b), smaller electric field enhancement occurs around the spheres when the nano gap is around 5 nm compared to the gap of 2.5 nm. It means that hotspots are formed between the silica and silver nanospheres and giant SERS enhancement can be obtained.
Fig. 10 Electric field (〈|E|〉2) distributions obtained from 3D FDTD calculations at wavelength 514 nm of (a) 2.5 nm gap (b) 5 nm gap. |
In the case of Ag@SiO2 using Ag hydrosol B, no noticeable intensity was observed for 10−12 M and 10−8 M due to the aggregated arrangement of Ag nanoparticles on monodispersed silica nanospheres. Fig. 11(a) shows normal Raman spectra of R6G for 10−8 and 10−4 M and the same on using silver sol A, while Fig. 11(b) and (c) show the SERS spectra of Ag@SiO2 using Ag hydrosol A and Ag hydrosol B respectively, where the maximum SERS is obtained for hydrosol A only. The use of Rhodamine 6G as a SERS probe using a 532 nm laser has been greatly discouraged, given the actual signal is coming from the so-called SER(R)S.47 The Rhodamine 6G is also in resonance with the laser, For confirmation of SERS we have taken the SERS spectra of R6G 10−11 molar concentration using 632 nm laser wavelength in Fig. 11(d). A similar work by Kudelski et al.48 shows that SERS effect is “switched on” in measurements with the red excitation radiation and the resonance Raman effect for R6G molecules is “switched off”. However the intensity recorded by them is very low for R6G using Ag@SiO2. In our case the peaks are shifted to ±5 cm−1 comparing to 514 nm wavelength and gives a much more high intense peak for R6G 10−11 M.
Hence it is concluded that the size of the Ag nanoparticles and the interparticle gap between silica and Ag nanoparticles are the primary factors for SERS enhancement. The enhancement factor was also calculated according to equation.26
The above calculations (see Fig. S11†) were done for the 20 μl R6G solution (1 × 10−3 M) and the R6G – absorbed on Ag@SiO2 (1 × 10−11 M, 20 μl) which were spread on the 1 × 1 cm2 prepare substrate. A laser spot area of 5 μm and power of (15 mW) was applied with an accumulation number of 1 s for all recordings. The Nbulk/Nsurf value is calculated to be 32.656 × 105 and ISERS/Ibulk are about 7.79 for the vibration peak at 1367 cm−1 (see Fig. S11†). The EF value is calculated to be about 7.79 × 108. Similarly we have also optimized the condition for lowest detection of 10−18 M based on their optical images as shown in the Fig. 12. In optical images we can easily able to identify the dye absorbance as shown in red color. The overall interpretation shows that when laser falls on red colored area we could expect enhanced Raman due to the linker molecule and charge transfer of dye into substrate. In case of 10−18 M the peaks were very weak but the spectra at 1367 cm−1 can be easily absorbed while the remaining peaks were shows very weak intensity. This confirms the contribution of highly monodispersed silica nanospheres for the SERS enhancement.
Fig. 12 Optical images of Ag@SiO2 nanospheres film using confocal Raman spectrometer (a) R6G 10−14 M (b) R6G 10−17 M (c) R6G 10−18 M. |
The designed substrates show good reproducibility that is confirmed through FESEM images (see Fig. S9†). A previous study on nanowires42 shows the tendency to form clusters after drying the analyte solution. But in the present study the nanospheres shows no bundling and clustering. The results show the good stability of nanospheres against the analyte. A substrate of 1 × 1 cm was dispersed with R6G with a molar of 10−11 and spectra were recorded for 30 spots to check the reproducibility of film (Fig. 13). The substrate shows highly intense and uniform peak over the substrate. The stability of prepared colloid was checked over the different substrates and different period of time which confirms the consistency of solution and film Fig. 13(d and e). Fig. 13(d and e) represents the SERS spectra of R6G over ITO and silicon substrate. This confirms that the present method is different from other techniques where the nanogaps formation is not defined over the substrate. The Fig. 13(b) clearly shows that the silver prepared using hydrosol A with a size of 15 nm exactly cling in between silica nanospheres due to the low nanogap between two spheres, whereas the bigger particle are not able to adhere inside the obtained gap (see Fig. S1†). So this confirms that the nanogaps formation in our substrate leads to good efficiency and reproducibility towards development of ultrasensitive SERS substrate. An Ag@SiO2 nanosphere for SERS application has been extensively analyzed in the present study, and it has been shown that a simple vertical deposition can be used to generate reproducible SERS substrates. The present method is technically sound and shows perfect morphology and designing procedure for the creation of hot spots. Moreover this method is of very low cost and is reproducible compared to other methods as shown in the comparative study (Table 1).
Substrate | Dye used and detection limit | Enhancement factor | Experimental method | Optical quality and remarks | Arrangement of silver over silica and its nanostructures | Ref. |
---|---|---|---|---|---|---|
Silica nanoparticles | R6G up to 10−5 M | 1.09 × 106 | Spin coating and vacuum deposition | Fair | Silver on monolayer silica. Structure not defined | 20 |
Polycrystal structure with low detection limit | ||||||
n-Type porous silicon nanostructures | R6G up to 10−10 M | — | Colloidal method | Poor | Randomly arranged Ag nanoclusters in porous silicon | 22 |
Difficulty in arrangement of pore diameter. Hot spots decrease while porosity increases | ||||||
Boron-doped single crystal silicon (sc-Si) wafers | R6G up to 10−15 M | — | Hydrothermal etching method | Fair | Ag/Si nanopillar like structure | 23 |
Silver agglomeration and interfacial strain. No confirmation of hotspots | ||||||
Silica colloidal microspheres | R6G up to 10−12 M | 1.68 × 107 | Colloidal method | Poor | Silica colloidal microspheres with silver | 24 |
Aggregated silver around silica and no proof for hot spots | ||||||
Silica wafer | R6G up to 10−18 M | 1016 | Modified colloidal | Fair | Ag nanocontacts onto silica | 25 |
Uniform sphere with agglomerated silver arrangement and no hot spots | ||||||
Ag@SiO2 nanospheres glass substrate | R6G up to 10−18 M | 7.79 × 108 | Vertical deposition (dip coating) | Excellent | Silver embedded silica nanospheres | Present Work |
Highly monodispersed spheres with maximum hot spots |
For the confirmation of SERS we have chosen another probe molecule melamine. Melamine is an organic chemical material and is mainly used to produce melamine-formaldehyde resins for glues, adhesives, and plastics. For boosting of protein content it has been used in dairy products such as milk.49 The present substrate shows the detection of melamine in liquid up to 10−8 molar concentration as shown in Fig. 14. Fig. 14 represents the SERS spectra of melamine in liquid for increasing concentration up to 10−8 M on to Ag@SiO2 substrate. The most prominent peak at 682 cm−1 is assigned to the ring breathing mode II and involves in-plane deformation of the triazine ring in melamine molecules.24
Fig. 14 SERS spectra of melamine enhanced by Ag@SiO2 (Ag hydrosol A) film for different molar concentrations. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5ra04355g |
This journal is © The Royal Society of Chemistry 2015 |