Frontier Institute of Science and Technology jointly with College of Science, State Key Laboratory for Mechanical Behavior of Materials, Xi'an Jiaotong University, Xi'an 710049, China. E-mail: ypdu2013@mail.xjtu.edu.cn
First published on 3rd December 2015
A new 3D composite electrocatalytic material is produced by growing WSe2 thin layers vertically on 2D reduced graphene oxide nanosheets. The material has improved electrode/electrolyte interactions and efficient catalytic properties due to the rich defects, a 3D hybrid configuration, and the direct integration of WSe2 onto the graphene sheets, which can significantly prevent the aggregation of WSe2 and promote the conductivity of the material. As demonstrated, the as-harvested WSe2/graphene hybrid exhibits excellent electrocatalytic activity in the hydrogen evolution reaction (HER), such as a low onset overpotential of −100 mV, a small Tafel slope of 64 mV per decade and outstanding stability.
As an important class of TMDs, tungsten selenide (WSe2) has a typical layered crystal structure, where each layer of W atoms is sandwiched between two layers of hexagonally close-packed Se atoms, and the atomic layers are stacked by weak van der Waals interactions.9 Additionally, WSe2 possesses a smaller band gap of ∼1.6 eV and exhibits excellent electrical transport performance in the category of TMD materials.10,11 Both theoretical calculations and experimental results have already highlighted that the HER activity of TMD materials arises from the active edge sites, indicating that the unsaturated dichalcogenide atoms on the edges play an important role in HER catalysis.12–15 However, the layered TMD materials can be easily re-stacked due to the intrinsic interlayer vdW attractions, as a result of reducing the active edge sites.16 Therefore, in order to further improve the catalytic performance, lots of efforts has been made to preserve the two-dimensional (2D) TMD nanostructures and introduce the desired defects, thus to design more active sites for promoting the HER activity. For instance, Cui's group developed layered vertically aligned 2D WSe2 nanofilms, exposing more active edge sites.17 He's group and Wang's group synthesized WS2(1−x)Se2x and WSe2 on carbon fibres, and assembled them as a working electrode, which exhibited promising HER performance owing to the abundant catalytic edge sites and enhanced charge transfer efficiency.18,19
In the present study, for the first time, we established a facile one-step colloidal synthesis method to fabricate a three-dimensional (3D) WSe2/rGO hybrid. This hybrid electrocatalyst was formed by the selective growth of WSe2 layers on 2D reduced graphene oxide (rGO) to obtain the assembled 3D configuration (Fig. S1, ESI†). Due to rGO as a unique support and the resulting 3D architecture, the aggregation of the WSe2 layers can be significantly prevented and thus facilitating electron transfer as well as exposing more catalytic edge sites. As a proof of concept application, the performance of the WSe2/rGO hybrid for the HER was evaluated (Scheme 1), which exhibited a superior HER activity with a low onset overpotential of −100 mV and a small Tafel slope of 64 mV per decade. Importantly, the HER activity of the WSe2/rGO hybrid can be maintained for at least 48 h without degradation under rigid acidic conditions.
![]() | ||
| Scheme 1 Schematic illustration of the 3D WSe2/rGO hybrid assembled from layered WSe2 anchored on graphene nanosheets and its application in the HER. | ||
:
5%) at 500 °C for 1 h.
:
1 by sonicating for 1 h to form a homogeneous ink. Then, 5 μL of the dispersion (containing 20 μg of catalyst) was loaded onto a rotating disk electrode (RDE) with a 3 mm diameter (loading ca. 0.285 mg cm−2). Linear sweep voltammetry with a scan rate of 2 mV s−1 was conducted in 0.5 M H2SO4 (purged with pure N2) using an electrochemical cell setup, with a saturated calomel electrode (Hg/HgCl2 in saturated KCl) as the reference electrode, a Pt plate as the counter electrode, and a RDE as the working electrode with a rotating speed of 1600 rpm. All the potentials were converted to values with reference to a reversible hydrogen electrode (RHE). Cyclic voltammetry was conducted at room temperature using the same standard three-electrode setup ranging from 0.3 to 0.4 V (vs. RHE) at a scan rate of 20, 40, 60, etc. mV s−1. The time-dependent current density curve of WSe2 and the WSe2/rGO hybrid was conducted under a static overpotential of −700 mV (vs. SCE) for the continuous operation of 48 h. Nyquist plots of the WSe2 layers and WSe2/rGO hybrid were measured on the AUTOLAB PGSTAT204 electrochemistry workstation in the frequency range from 0.1 Hz to 100 kHz at an open circuit potential with 10 mV as the amplitude potential. The WSe2/rGO hybrid and pure WSe2-coated CFPs (1 cm2, catalyst loading 1 mg) were used as working electrodes to collect chronoamperometry data at the applied potential of −0.7 V vs. SCE.
:
Se in the as-formed WSe2 (W
:
Se = 1
:
2).
The high-resolution TEM (HRTEM) images taken from different positions on the WSe2 layers grown on rGO show clear lattice fringes, demonstrating the as-obtained WSe2 layers are of high crystallinity (Fig. 2a and b). As seen from the planar orientation (Fig. 2a), WSe2 shows lattice fringes with interplane spacings of ∼0.28 nm and the fast Fourier transformation (FFT) pattern (inset of Fig. 2a) exhibits six independent diffraction arcs, which can all be indexed to the (100) plane of hexagonal (2H-type) WSe2. Moreover, the present diffraction arcs of the FFT pattern can be attributed to the quasiperiodic structure with rich defects.26 Meanwhile, the layered structure with interlayer spacings of ∼0.64 nm and ∼0.28 nm can be observed from the vertically stacked WSe2 layers (Fig. 2b), corresponding to the (002) and (100) plane of WSe2, respectively, while the FFT pattern (inset of Fig. 2b) reveals the orientation of the layers along the <001> direction. Importantly, the HRTEM images also demonstrate that there are lots of defects (highlighted in the circular areas of Fig. 2a and b) in the present WSe2 layers, which are expected to serve as active sites to improve the HER catalytic performance.26,27–29 The corresponding crystal structure model shown in Fig. 2c–e can foster the understanding of the as-harvested WSe2 structure illustrated in the HRTEM images. Viewed from the <001> direction (Fig. 2d), WSe2 holds the graphene-like structure and the (100) plane is labeled, which is consistent with the HRTEM image shown in Fig. 2a. Moreover, viewed from the <010> direction (Fig. 2e), just like the vertically standing WSe2 layers, the (100) and (002) planes are marked and also agree well with the HRTEM image shown in Fig. 2b.
The detailed structure and chemical state for the WSe2/rGO hybrid were investigated using Raman spectroscopy and X-ray photoelectron spectroscopy (XPS). Fig. 3a shows the Raman spectrum of the WSe2/rGO hybrid; due to the small energy difference between the A1g (out-of-plane) (253 cm−1) and E12g (inplane) mode (250 cm−1), there is only one broad peak situated from 200 to 400 cm−1.30 Meanwhile, the characteristics of the graphene Raman shift for D, G, and 2D bands can be observed in the WSe2/rGO hybrid (Fig. 3a).31 The XPS spectrum of W is shown in Fig. 3b, and the binding energies of W 4f7/2 and W 4f5/2 located at 32.3 and 34.5 eV indicated that the elemental chemical state of W is mainly quadrivalent for the WSe2/rGO hybrid.32 Meanwhile, the small peak located at 37.7 eV is ascribed to the core levels of W 5p3/2 from WO3 due to the partial oxidation of the WSe2 layers.17 Two intense peaks at 54.1 and 54.9 eV (Fig. 3c) attributable to the core levels of Se 3d5/2 and Se 3d3/2, respectively, are characteristic of Se2− of the WSe2/rGO hybrid.33,34 The C 1s XPS signal shown in Fig. 3d demonstrated that there was a trace amount of oxygen content in the WSe2/rGO hybrid, confirming the reduction of GO to rGO.35
In the present synthesis, the combination of capping ligands (OA and OM) and the amount of the Se powder precursor were found to play crucial roles in the formation of high-quality WSe2 products. For example, fixing the amount of solvent (20 mmol) and the mole ratio of (NH4)2WO4 and the Se powder ((NH4)2WO4
:
Se = 1
:
3), when using 0.2 mmol of (NH4)2WO4, 0.6 mmol of Se and pure OM as a solvent at 280 °C for 60 min, the pure phase WSe2 products were obtained (Fig. 1a). Under the same reaction conditions, except using OA as the solvent (e.g. OM
:
OA = 1
:
1 and pure OA), the harvested products possessed a layered structure (Fig. S3a and b, ESI†), but coexisted with a small amount of tungsten oxide (WO3) (Fig. S3c, ESI†). In addition, when the mole ratio of (NH4)2WO4 and the Se powder was larger than 1
:
3 (e.g. 1
:
2, 0.2 mmol of (NH4)2WO4, 0.4 mmol of Se) in pure OM at 280 °C for 60 min, the as-prepared samples also contained considerable impurities with nanorod morphologies (Fig. S4a and b, ESI†). To conclude, after a series of condition based experiments, we found that high-quality WSe2 layers can be obtained in 20 mmol of OM solvent at a temperature of 280 °C for 60 min under the precursor concentration of 0.2 mmol of (NH4)2WO4 and 0.6 mmol of Se powder, which can elegantly maintain the balance between nucleation and growth stages (Fig. 1b and S2a, ESI†).
The HER electrocatalytic performance of the as-prepared WSe2 layers and WSe2/rGO hybrid were investigated using a standard three-electrode setup with the same loading value of 0.285 mg cm−2 on a rotating disk electrode (RDE) in 0.5 M H2SO4 electrolyte degassed with N2 (experimental section). As shown in Fig. 4a, the polarization curves (iR corrected) show the current density versus voltage (J versus V) for the comparison of the WSe2 layers and WSe2/rGO hybrid along with the Pt/C (15%) samples. As depicted in Fig. 4a, only rGO had no HER activity, hinting that the core catalysts were the WSe2 layers. Compared to the pure WSe2 layers, the onset potential of the WSe2/rGO hybrid shifted from −160 mV to −100 mV and significant H2 evolution (J = 10 mA cm−2) was observed at −180 mV, which was much smaller than WSe2 (−307 mV) vs. RHE, suggesting the excellent catalytic activity of the WSe2/rGO hybrid. In order to further study the HER electrocatalytic performance of the WSe2/rGO hybrid, WSe2 layers physically mixed with rGO (WSe2 + rGO) having the same ratio as the WSe2/rGO hybrid were also investigated, which exhibited a much lower HER catalytic activity (Fig. S5a, ESI†). The superior HER catalytic performance of the WSe2/rGO hybrid compared to WSe2 + rGO may be due to the improved charge transfer efficiency between the WSe2 layers and rGO.12,36 In addition, the HER electrocatalytic activities of the WSe2/rGO hybrids with different WSe2 to rGO content ratios were measured (Fig. S5b, ESI†). When the loading density of WSe2 on rGO was higher (0.2 mmol of WSe2/10 mg of rGO), a relatively lower catalytic performance was obtained, probably due to the lower efficiency of charge transfer.26,37 On the contrary, when the loading density of WSe2 on rGO was lower (0.2 mmol of WSe2/30 mg of rGO), an inferior catalytic performance resulted from the lower loading density of the core catalysts of WSe2. Thus, 0.2 mmol of WSe2 loaded on 20 mg of graphene (0.2 mmol of WSe2/20 mg of rGO) is the optimized content ratio for fulfilling the best HER performance.
The promising enhancement in HER activity (Fig. 4b) was apparent by comparing the Tafel slopes of the WSe2/rGO hybrid (64 mV per decade, after iR correction) with those of pure WSe2 layers (126 mV per decade, after iR correction), demonstrating that the kinetic speed of electrochemical hydrogen evolution for the WSe2/rGO hybrid was much faster than for the pure WSe2 layers. This Tafel slope was also comparable to or even lower than the previously reported WSe2-based HER catalysts (Table S1†). Generally, a Tafel slope includes three principal steps in converting H+ to H2 in the HER:12,38–40
| H3O+ + e–M ↔ H–M + H2O (Volmer reaction) | (1) |
| 2H–M ↔ H2–M + M (Tafel reaction) | (2) |
| H3O+ + e–M + H–M ↔ H2–M + M + H2O (Heyrovsky reaction) | (3) |
Apart from the current density and Tafel slope, the stability of the catalyst is another important criterion for the HER. The long-term stability of the WSe2 layers and WSe2/rGO hybrid catalysts is conducted by means of continuous HER at the static overpotential of −0.7 V vs. SCE in 0.5 M H2SO4 for 48 h. The WSe2 layers and WSe2/rGO hybrid catalysts are loaded on carbon fibre paper (CFP) with a high catalyst loading concentration of 1 mg cm−2 (Experimental section). As shown in Fig. 4c, the current density of the WSe2/rGO hybrid modified CFP electrode increases gradually at the initial ∼2 h and then remains stable even after a long period of 48 h. Furthermore, digital photos (inset of Fig. 4c) taken of the WSe2/rGO hybrid modified CFP electrode at the start and end of the durability test, show the vigorous effervescence of H2 bubbles (Movie 1, ESI†). Remarkably, the XPS spectra of the WSe2/rGO hybrid after the HER for 48 h show no obvious change in the chemical state of both the W and Se elements (Fig. S6a and b, ESI†), indicating that the WSe2/rGO hybrid catalysts are rather stable in a rigid acidic environment for a long time. In comparison, under the same HER conditions, the pure WSe2 exhibited a relative fluctuation in HER activity after 11 h (Fig. S7, ESI†).
The smaller (64 mV per decade) Tafel slope, lower onset potential (−100 mV) and outstanding stability verify that the WSe2/rGO hybrid can be an effective electrocatalyst for the HER. We also performed electrochemical impedance spectroscopy (EIS) of the WSe2 layers and WSe2/rGO hybrid to investigate the electrode kinetics for the HER. The Nyquist plots of the WSe2 layers and WSe2/rGO hybrid samples are compared (Fig. 5a) and fitted to an equivalent circuit (Fig. S8, ESI†), where a constant phase element (CPE) is employed. As displayed in Fig. 5a, the Nyquist plots reveal a decrease in the charge-transfer resistance (Rct) for the WSe2/rGO hybrid (40.8 Ω) compared to the pure WSe2 layers (81.7 Ω), indicating a smaller reaction resistance and higher catalytic activity for the HER in acid solution for the WSe2/rGO hybrid electrode. In addition, as shown in the inset of Fig. 5a, the WSe2/rGO hybrid also exhibited a smaller Rs (0.4 Ω) than the WSe2 layers (0.8 Ω), demonstrating that our one-pot synthesis strategy for the growth of the WSe2 layers on graphene could also improve the electrical contact at the interface of the electrode.
We further compared the electrochemical surface area (ECSA) of the WSe2 layers and WSe2/rGO hybrid samples by measuring the double-layer capacitance (Cdl). Fig. 5b and c show the typical cyclic voltammograms (CVs) of the WSe2 layers and WSe2/rGO hybrid, respectively, taken with various scan rates (20–200 mV s−1) in the region of 0.3–0.4 V (vs. RHE) in 0.5 M H2SO4. Current density differences (ΔJ = Ja − Jc) at 0.35 V (vs. RHE) are then plotted against the scan rate. The electrochemical double-layer capacitance values, which are equivalent to half of the linear slopes in Fig. 5d, are used to represent and compare the ECSA of the WSe2 layers and WSe2/rGO hybrid. It is noteworthy that the Cdl of the WSe2/rGO hybrid (3.1 μF) is much higher than that of the WSe2 layers (1.4 μF), suggesting that the WSe2/rGO hybrid possesses a much larger active surface area and more active sites for hydrogen production.8,41
Three possible reasons could be responsible for the excellent HER performance of the 3D WSe2/rGO hybrid nanostructures. Firstly, the WSe2 layers are vertically grown on rGO, which can effectively reduce the agglomeration of the WSe2 layers, maximally exposing the active edges and reducing the solid–gas interaction. Secondly, the charge transfer efficiency at the electrode interface is greatly promoted through combining with the highly electrically conductive rGO. The last one is the defect-rich structure of the WSe2/rGO hybrid, which contributes to the additional catalytically active sites.
Footnote |
| † Electronic supplementary information (ESI) available: SEM and TEM images of GO and optimal conditional experiments, and the comparison of HER performance for different ratio of WSe2/rGO hybrid catalysts. See DOI: 10.1039/c5qi00216h |
| This journal is © the Partner Organisations 2016 |