Antonio
Iborra-Torres
a,
Matej
Huš
bcd,
Kiem
Nguyen
e,
Antonis
Vamvakeros
fg,
Muhammad Tariq
Sajjad
e,
Steven
Dunn
e,
Myrjam
Mertens
h,
Simon
Jacques
f,
Andrew M.
Beale
fgi,
Blaž
Likozar
b,
Geoffrey
Hyett
a,
Suela
Kellici
e and
Vesna
Middelkoop
*h
aDepartment of Chemistry, University of Southampton, Southampton, SO17 1BJ, UK
bDepartment of Catalysis and Chemical Reaction Engineering, National Institute of Chemistry, SI-1001 Ljubljana, Slovenia
cAssociation for Technical Culture of Slovenia, Zaloška 65, SI-1001 Ljubljana, Slovenia
dResearch Institute, Conservation Centre, Institute for the Protection of Cultural Heritage of Slovenia, Poljanska 40, SI-1000 Ljubljana, Slovenia
eLondon Centre for Energy Engineering, School of Engineering, London South Bank University, London SE1 0AA, UK
fFinden, Building R71, Harwell Campus, Oxfordshire, OX11 0QX, UK
gDepartment of Chemistry, University College London, London WC1H 0AJ, UK
hSustainable Materials Management, Flemish Institute for Technological Research (VITO), B-2400 Mol, Belgium. E-mail: vesna.middelkoop@vito.be
iResearch Complex at Harwell, Rutherford Appleton Laboratory, Harwell Science and Innovation Campus, Didcot, Oxon OX11 0FA, UK
First published on 13th March 2023
Organic pollutants in water are a major concern for the environment and human health, and require urgent attention. Here, we developed for the first time monolithic structures by 3D printing of perovskite metal oxynitride, SrNbO2N, for photocatalytic degradation of organic pollutant in water. Advanced, synchrotron-based XRD-CT measurements were employed to gain structural insight into photocatalyst formulation and assess the fidelity of design in terms of both the chemical and physical form of the photocatalysts to be imaged. Our 3D printed material showed excellent photocatalytic activity, degrading 100% of methylene blue (MB) as well as good stability for three cycle operations. This is due to high adsorption of the 3D printed oxynitride towards MB which enhanced its photoredox reactivity. It is also evident from the excellent charge transfer demonstrating a charge transfer rate of (1.5 ± 0.2) × 108 s−1. We performed Time-Dependent Density Functional Theory (TD-DFT) calculations to understand the photocatalyst structure and degradation pathways. Our calculated band gap (at Γ) of 1.88 eV is in good agreement with the experimental values. We found that the highest valence bands were contributed by N p orbitals and the lowest conduction bands corresponded to Nb d orbitals offering avenues for fine-tuning the band gap. Hence, the ability to tailor photocatalyst monoliths by 3D printing renders their water treatment application more facile compared to their powder suspension counterparts.
The mechanism of photocatalytic degradation typically involves the generation of electron–hole pairs by absorbing photons from light, followed by the transfer of these charges to the surface of the photocatalyst, where they can participate in redox reactions. Perovskite oxynitrides have been shown to have a wide band gap and can be excited by UV light, leading to the generation of electron–hole pairs. Fig. 1 illustrates how these charges, when reacting with water molecules, lead to the production of reactive oxygen species (ROS), such as hydroxyl radicals (˙OH). The ROS have the ability to oxidize and degrade organic compounds, including dyes.1 These photocatalytic properties (including a visible light absorption band) make perovskite oxynitrides (for example Sr, Nb and Ti based) promising materials for water splitting2 and the degradation of organic pollutants and biological contaminants in water3–5 including degradation of organic compounds such as acetone (LaTi(O,N)3),6 methyl orange (CaTaO2N;7 CaNbO2N and SrNbO2N)8 and methylene blue,9 among others.10
Fig. 1 Generation of reactive oxygen species (ROS) and process of photo-oxidation of an organic pollutant. Step (a) is absorption of a photon to generate an excited electron–hole pair which can then migrate to the surface of the photocatalyst particle, where (b) the electron can then reduce atmospheric oxygen to the more labile superoxide radical. In step (c) the superoxide radical and subsequent ROS can oxidise an organic pollutant to CO2. The holes can form surface bound hydroxyl radicals which can also directly oxidise organic molecules.1 |
Previously we reported8 seven tantalum and niobium oxynitrides ABON2 (where A = Ca, Sr, Ba; B = Nb or Ta) for self-cleaning reactions using dichloroindophenol (in the presence of a sacrificial electron donor) and stearic acid as test pollutants. Although all of the oxynitride samples showed the ability to degrade the test pollutant, they did so poorly with at best 1.5% of the dye being degraded after 3 hours. However, after decorating the oxynitride with co-catalyst particles of cobalt oxide, a significantly higher activity was observed. All of the oxynitrides were active, with the most active being SrNbO2N that degraded 25% of the dye after 3 hours – a twenty fold increase compared to the sample without the co-catalyst.
In recent years, there have been a number of examples of 3D structured photocatalytic reactors using TiO2 deposited on a solid foam.11,12 No examples of 3D printed oxynitride-based photocatalysts have been reported to date, only a very limited number of other photocatalyst compositions.13–16 The photocatalytic microreactors based on microfluidic technology that use a catalyst dispersed in powder form, have been extensively reported.17 However, it requires an additional step to separate the catalyst from the products, thus leading to an increase in the experimental cost and time. 3D printed photocatalytic structures can resolve the challenges associated with the immobilisation of the photocatalyst as well as its recovery and ease of product separation. In addition, 3D printing allows complex shapes and optimised geometries to be easily tailored, thereby facilitating the flow patterns and efficient light management. One of the major advantages of the orderly-structured micro-channel catalytic or adsorbent beds over randomly powder packed beds is an increased mass transfer, reduced pressure drop and higher selectivity per cubic metre of reactor volume, by their controlled porosity and controlled product distribution.18–21 Examples of the development and characterisation of the 3D printed microchannel catalysts can be found in our previous work.22–25
This work describes the development, characterisation and modelling of oxynitride SrNbO2N material that was 3D printed and employed for the photodegradation of a simulant pollutant (methylene blue dye in aqueous solution) under simulated solar light irradiation. For that, a printing ink containing SrNbO2N was first formulated followed by the deposition of stacked fibres using direct ink writing (DIW) to form a monolithic photocatalyst. This monolith was evaluated for its efficiency to generate reactive oxygen species and to degrade pollutant (MB) in aqueous solution. It should be noted that relevant scientific literature suggest that MB is a suitable standard to test the photocatalytic performance of materials.26 The 3D printed monolith showed excellent photocatalytic activity with 100% degradation of pollutant within just 3.5 hours. The photophysical study shows excellent charge transfer between the 3D printed perovskite (SrNbO2N oxynitride) structure and MB. The DFT calculations of photocatalytic structure and degradation pathways show good agreement with experimental data.
The solution was then heated at 120 °C for 90 minutes to allow the complete evaporation of the methanol, resulting in formation of a transparent resin. The gel containing the metal cations was placed into an alumina crucible and pre-calcined in air for 1 h at 350 °C, followed by 1 h calcination at 650 °C and finally 2 h at 800 °C at a constant heating rate of 10 °C min−1 at each step. The heating cycle converted the gel into a white metal oxide powder. The resultant oxide powder in the alumina crucible was heated (3 °C min−1 ramp rate) and nitrided inside a tube furnace under an ammonia flow (of 250 mL min−1 anhydrous, BOC, 99.98%) for 15 h at 850 °C. The SrNbO2N product was cooled down under flowing ammonia to avoid its re-oxidation.
The 3D printed photocatalysts were subsequently subjected to a heat treatment and ammonolysis to remove the organic binder component and obtain the final desired structure and photocatalytic properties. For the removal of the organic binder component, the 3D printed monolith was heated under a flow of air (250 mL min−1) at 650 °C for 2 hours (heating rate of 10 °C min−1).
For the deposition of the Cobalt oxide co-catalyst, the 3D printed monolith was immersed in 1.12 mL of a 0.009 M Co(NO3)2 (Sigma-Aldrich, 98%) water solution aiming at 2% wt loading. The suspension was treated for 5 minutes in an ultrasound bath and heated to promote the evaporation of the water. The resulting monolith was treated under flowing ammonia (250 mL min−1) for 15 hours at 850 °C (heating rate of 3 °C min−1). Finally, the co-catalyst was activated via mild oxidation in air at 200 °C for 1 h.
The analysis of diffraction data was performed with the TOPAS v7 software33 on a voxel-by-voxel basis. A pseudo-Voigt peak shape function calculated after the analysis of the CeO2 calibrant pattern was used for diffraction data. The data were also analysed using the Direct Least-Squares Reconstruction (DLSR) approach34 which overcomes the parallax artefact. Due to the memory expensive requirements of the DLSR approach, the data had to be downscaled by a factor of two to 165 × 165 pixels. This means that the pixel size in the reconstructed DLSR maps corresponds to 200 microns. The downscaled sinograms (containing parallax artefact) were used to reconstruct images using the conventional approach and perform analysis using the Rietveld method. To stabilize the DLSR refinements, the SrNbO2N scale factor map obtained from the conventional analysis was used as an input to the DLSR. A mask was created based on the SrNbO2N scale factor map which allowed us to decrease the number of structures needed to be refined. A 3XS Data Science Workstation C264X2 with 2× Intel Xeon Silver 4216 and 350 GB RAM was used to perform the refinements for both the conventional approach (FBP + Rietveld) and the DLSR approach.
Characteristically, the 3D printed photocatalyst (2.29 g) was suspended in MB aqueous standard solution (0.04 mM, 0.4 L) in a photocatalytic reactor (glass beaker, Corning Pyrex Griffin). To ensure the establishment of an adsorption–desorption equilibrium, the reaction mixture was agitated in the dark for 30 minutes. It was kept at a distance (27 cm) from the light source and constantly agitated throughout the photocatalytic process. The sample was irradiated for 210 minutes. During the irradiation procedure, aliquots were taken at 30 minutes intervals, and analysed using UV-vis spectrophotometry (Shimadzu UV-1800) to determine MB photodegradation (by changes observed at λabs = 665 nm). A calibrated correlation between the measured absorbance and its concentration was used for the quantitative determination of MB. The rate of direct degradation of MB was measured in the absence of the catalyst and was found to be negligible. The adsorption coefficient, qt (the adsorbed mass (mg) of MB per mass (g) of catalyst, at time (t) was calculated according to the following equation):35
(1) |
To assess the catalyst's efficiency over time, the 3D printed monolith was recycled and then re-exposed to irradiation, using the same testing approach as previously described. The sample was recovered after each run by periodically washing it with ethanol followed by drying. To investigate the photocatalytic degradation of MB by the 3D photocatalytic monolith the following parameters were considered:, the initial contaminant (dye) concentration, initial pH solution, the presence of oxidants and electron acceptors, photocatalyst concentration, photocatalyst particle size, reactor/structured matrix dimensions, reaction temperature as well as light intensity.
Intermediates were geometrically optimized until the forces on all atoms dropped below 1.5 × 10−5 hartree bohr−1. Vibrational analysis was performed to confirm that stable stationary points were found. Photocatalytic degradation of MB was modelled as an attack of the OH* radical on the ground state and excited MB molecule in solution.
For catalyst structure calculations, plane-wave DFT as implemented in VASP 5.4.1 was used.45,46 Preliminary calculations, including geometry optimizations, were performed with a GGA functional (PBE) with the projector-augmented wave method (PAW).47,48 To account for d electrons of niobium, a Hubbard value of 3 eV was used in the DFT+U approach,49 although the effect of this value is small.50 For the plane waves expansion, a cut-off of 500 eV was employed. Dispersion interaction was described with the Grimme D3 correction. For band structure and band gap evaluation, single point calculations with a hybrid functional (HSE06) were performed on the PBE-level optimized structures.51 A gamma centered Monkhorst–Pack mesh 11 × 11 × 7 was sufficient to describe a 5.81 × 5.81 × 8.18 Å unit cell, which agrees well with the experimental determination (5.71 × 5.71 × 8.10 Å).50,52,53
Fig. 3 Reconstructed XRD-CT images of the 3D printed photocatalyst based on the Rietveld analysis of four isolated SrNbO2N peaks (single phase model) using the conventional approach (left) and the DLSR approach (right) shown in each of the three sub-figures: (a) lattice parameter a (LPA) maps (colour bar axis in Å), (b) lattice parameter c (LPC) maps (colour bar axis in Å), (c) crystallite (CLS) maps (colour bar axis in nm). Every pixel in the reconstructed XRD-CT image corresponds to a single diffraction pattern. The pixel size in the reconstructed DLSR maps corresponds to 200 μm as the data had to be downscaled by a factor of two to 165 × 165 pixels. Accompanying figures can be found in the ESI† (see Fig. S1 and S2). |
The XRD-CT data on the left-hand side of each sub-figure was obtained using the conventional approach that presents the reconstructed images based on the FBP algorithm and the analysis of the local diffraction patterns which is based on the Rietveld method. This type of analysis can lead to accurate scale factor and weight fraction maps for the various crystalline components in the sample despite the parallax artefacts present in the data. One global scale factor was refined for the SrNbO2N phase, i.e., the distribution of the component was forced to be the one obtained from the conventional approach. However, a scale factor was applied to this map which was refined during the DLSR analysis (presented on the right hand-side of each sub-figure). The reconstructed maps of the lattice parameters and crystallite size of the SrNbO2N phase were refined spatially. For both the conventional FBP-Rietveld and DLSR approaches, a selected region of the diffraction patterns was used: Q = 2.01–2.3, 3.58–3.93, 4.74–5 and 5.6–5.9 Å−1. These regions contained isolated SrNbO2N diffraction peaks (including the (112), (204), (420), (116), (316) and (512) reflections) which allowed to avoid using the difficult-to-model Al2O3 support phase in the refinement process. The weighted profile R-factor (Rwp) is ca. 8–9% for most pixels. The overall Rwp for the global DLSR refinement is similar too, at 8.8%. ensuring that the comparison of the reconstruction algorithms was not biased.
It can be observed that for the conventional approach to XRD-CT, image analysis leads to more uniform and underestimated values for the lattice parameters while local inhomogeneities can be observed across the sample by the DLSR approach. The DLSR approach accounts for the loss of physico-chemical information associated with diffraction peak shape and position and directly yields the varying lattice parameter and crystallite size throughout the scanned cross section. The values of the lattice parameters a and c vary from 5.60–5.80 and 8.04–8.32 Å respectively. These values are in agreement with lattice parameters results obtained from the bulk sample by the conventional XRD measurements (presented in ESI,† Fig. S3 and S4): 5.71 and 8.12 Å for a and c respectively. Both the conventional and XRD-CT diffraction patterns were indexed with the space group I4/mcm.54 The DLSR approach yields lower and more uniform values for the crystallite size. Fig. S2 in the ESI† shows a histogram of the crystallite size distribution obtained from the DLSR CLS map.
Experiment | Rate constant (1014 s−1) | MB photodegradation (%) | q t |
---|---|---|---|
1st photocatalytic activity | 4 | 100 | 2.23 |
2nd photocatalytic activity | 3 | 96 | 2.14 |
3rd photocatalytic activity | 0.6 | 62 | 1.38 |
4th photocatalytic activity | 0.5 | 56 | 1.26 |
5th photocatalytic activity | 0.2 | 32 | 0.70 |
The 3D printed monolith demonstrated excellent photocatalytic activity, with ca. 100% degradation of MB in the allotted 210 minutes time period and a significant two-fold enhancement when compared to our previously reported work, in which we tested photodegradation of blue DCIP dye in the presence of a sacrificial electron donor.8 The 3D printed oxynitride also exhibited adsorption toward MB, allowing it to effectively react with photogenerated active species on the surface of the 3D printed oxynitride, enhancing photoredox activity. It should be noted that, a control experiment carried out under the same conditions but without the addition of photocatalyst, provided an assessment of the extent of direct photochemical reaction of MB which was proved to be negligible when compared with that in the presence of the catalyst (see Fig. S11 in the ESI;† Fig. S12, ESI† shows the absorption spectra of MB degradation in the absence of the catalyst). Irradiance curve (irradiance readings as a function of wavelength) for the light source used in the experiments shown Fig. 4–6 can be found in ESI,† Fig. S13. The Tauc plot for the SrNbO2N photocatalyst used as a conventional method for extracting the band gap of a material is presented in ESI,† Fig. S14.
One important feature associated with the usage of photocatalysts is long term stability and their cyclic use. To evaluate the efficiency over time, a series of experiments were conducted where the 3D printed monolith was recycled and subjected to photocatalytic testing under solar light. The change in methylene blue concentration is shown in Table 1. The 3D printed monolith exhibited good stability for 3 cycle operations, reaching an adsorption plateau for cycles 2 and 3, while remaining efficient in terms of photocatalytic degradation of MB.
It should be noted that cobalt oxide, when used (even in low concentrations) as a co-catalyst with perovskite oxynitrides, can enhance the photocatalytic activity of the perovskite oxynitride by acting as a promoter and providing additional active sites for the adsorption and activation of reactants. The CoOx species (shown in Fig. S8, ESI†) can also facilitate the transfer of electrons and holes between the perovskite oxynitride and dye molecules, leading to more efficient degradation as previously described by the authors.8
We determined the lifetimes by fitting the data with multi-exponentials. The equation and parameters are provided in the ESI† (see eqn (S1) and Table S1).
The charge transfer can be quantitatively determined from the additional rate of decay in the presence of MB (quencher).55,56 We determine this rate of quenching by taking the differentiation or the slope of the natural logarithms of the PL ratio of 3D monolith with MB and without MB (Fig. 6) using:
(2) |
The resulting charge transfer rate of (1.5 ± 0.2) × 108 s−1 after first photocatalytic activity, (5.0 ± 0.5) × 108 s−1 after 2nd photocatalytic activity, (5.6 ± 0.6) × 108 s−1 after 3rd photocatalytic activity experiment, (1.2 ± 0.2) × 109 s−1 after 4th photocatalytic activity experiment and (1.3 ± 0.1) × 109 s−1 after 5th photocatalytic activity experiment.
In studying photodegradation, we are most interested in the changes in reactivity upon the excitation of methylene blue. From the natural bond order (NBO) analysis, a charge redistribution is noticeable. In the ground state, the S6 atom is positively charged +0.485e, while N5 and N7 are negatively charged with −0.366e and −0.421e, respectively. As shown in Fig. 8, the N5 atom is the most electropositive part of the molecule. In the excited state, however, the electrons accumulate in the hetero-ring, increasing the charge of S6 to +0.395e and N5 to −0.515e. On the other hand, the charge density on the amine group and outer aromatic rings slightly decreases.
Fig. 8 (left) Electrostatic potential of methylene blue in ground state shows and (right) differential electron density between the excited and ground state. |
While listed numerically in Table 2, this is more easily shown as a differential electron density between the excited and ground state in Fig. 8. It demonstrates that as electrons flow towards the excited molecule, the N5 becomes more reactive.
Site | Atom charge in atomic units | |
---|---|---|
Ground state | First excited state | |
1 | −0.301 (−0.048) | −0.245 (−0.007) |
1a | −0.157 | −0.207 |
2 | +0.281 | +0.247 |
3 | −0.268 (−0.018) | −0.231 (+0.019) |
4 | −0.125 (+0.123) | −0.172 (+0.075) |
4a | +0.093 | +0.196 |
5 | −0.366 | −0.515 |
6 | +0.485 | +0.395 |
7 | −0.421 | −0.367 |
A more quantitative measure of the regioselectivity are the Fukui functions, which indicate the change in electron density when the number of electrons in the molecule changes. The Fukui function for the nucleophilic attack in the ground state shows the highest regioselectivity at N5 and N7 and moderate regioselectivity at C2 and C4a. Conversely, the electrophilic attack is most likely at C1 and C3. The radical attack will most likely proceed on N5, C4a, C1 and C3.
In the excited state, the electron density is perturbed (see Fig. 8), which also affects the regioselectivity. The nucleophilic attack is still most likely at N5, but C3 and N7 also show non-negligible reactivity, while the electrophilic attack is centred on N5 and S6. The excited molecule is susceptible to a radical attack on N5, S6, C1, C1a, C2 and C4. The Fukui functions are plotted in Fig. 9.
Fig. 9 Fukui functions of MB for the nucleophilic (f+), electrophilic (f−) and radical attack (f0) in the ground state (GS) and the first excited state (ExS). |
As shown in Table 3, there is considerable difference in the activity of different sites in MB. OH* will most favourably abstract a hydrogen atom from the methyl group, which activates the cascade of N-demethylation. Other (aromatic) hydrogen atoms are not likely to be abstracted (152–160 kJ mol−1). Alternatively, OH* can bind to carbon atom, most favourably to C1, followed by C3 (relative energy +51 kJ mol−1 with respect to C1-intermediate), C4a (+63 kJ mol−1) and C4 (+81 kJ mol−1). The heteroatoms (N5, S6 and N7) are least likely to be attacked by the OH* radical. This shows that in the ground state, the degradation by the OH* radical begins with N-demethylation, while the aromatic ring structure is attacked at the C1 or C3 site. However, this changes upon excitation.
Site | Energy (relative to the most stable intermediate) in kJ mol−1 | |
---|---|---|
Ground state | First excited state | |
1-OH | +51 | +171 |
1a-OH | +98 | +207 |
2-OH | +102 | +99 |
3-OH | +63 | +129 |
4-OH | +81 | +289 |
4a-OH | +74 | +160 |
5-OH | +115 | +65 |
6-OH | +137 | +163 |
7-OH | +141 | +231 |
1-H abstraction | +153 | +198 |
3-H abstraction | +152 | +206 |
4-H abstraction | +160 | +206 |
Methyl-H abstraction | 0 | 0 |
While MB is flat in the ground and excited state, its intermediate with OH* is planar in the ground state but assumes a bent geometry in the first excited state (see Fig. 10). This has consequences for the degradation pathways, as well. While the attack on the methyl group with hydrogen abstraction remains most favourable, the reactivity of ring sites is changed. For instance, while poorly reactive in the ground state, N5 is preferentially attacked by OH* when MB is in the first excited state. The reactivity of the aromatic carbon atoms does not change as drastically with C3, C4a and C4 remaining most reactive (but less than the aromatic nitrogen atom N5). Experimentally, it was confirmed previously that N-demethylation proceeds concomitantly with the degradation of the phenothiazine structure of MB,58 which is in line with our calculation of similar energies for the OH attack on C1 and hydrogen cleave from N-methyl (difference of 13 kcal mol−1), as shown in Table 3.
Once a hydrogen atom is cleaved from the methyl group, N-demethylation rapidly follows, yielding azure B, azure A, azure C and thionine with three, two, one and no methyl groups, respectively.59 Since the mechanism of radical N-demethylation is analogous for all methyl groups, we present the calculations for one cascade, only.
We model hydrogen atoms to be cleaved off by an impacting OH* radical, yielding H2O in the process. The results show that C–H bond cleavages are more exothermic than C–N bond cleavage, meaning that N-demethylation proceeds stepwise through –NR-CH3, –NR-CH2*, –NR-CH, –NR-C*, –NR*, and –NRH intermediates. In the last step, the –NR* radical does not abstract a hydrogen atom from a water molecule (this reaction would be endothermic) but instead reacts with a new MB molecule in a new exothermic reaction, propagating the reaction chain by converting it to –NR-CH2*. The mechanism and energetics in the ground and excited states are similar (see Table 4 and Fig. 11).
Reaction | Energy in kJ mol−1 | |
---|---|---|
Ground state | First excited state | |
Ar–NCH3CH3 + OH* → Ar–NCH3CH2* + H2O* | −179 | −201 |
Ar–NCH3CH3 + OH* → Ar–NCH3* + CH3OH | −66 | −134 |
Ar–NCH3CH2* + OH* → Ar–NCH3CH + H2O* | −98 | −55 |
Ar–NCH3CH2* + OH* → Ar–NCH3 + CH2OH* | +21 | −25 |
Ar–NCH3CH + OH* → Ar–NCH3C* + H2O* | −88 | −284 |
Ar–NCH3CH + OH* → Ar–NCH3* + CHOH | −43 | −132 |
Ar–NCH3C* + OH* → Ar–NCH3* + COH | −128 | −22 |
Ar–NCH3* + H2O → Ar–NHCH3+ OH* | +100 | +175 |
Ar–NCH3* + Ar–NCH3CH3 → Ar–NHCH3+ Ar–NCH3CH2* | −78 | −26 |
In SrNbO2N (and other perovskite oxynitrides), niobium atoms are in octahedral sites surrounded by nitride and oxide anions. Sr atoms are at the A sites, Nb atoms are at the B sites (ABO3). The position of nitrogen and oxygen anions can vary and several isomers are possible,61 which has already been extensively studied with first-principle methods.50,62–65 Our results show that nitrogen atoms assume the equatorial cis positions, which is consistent with the findings of Stotskyi et al.50
For an additional insight into the origin of its electronic properties, we calculated the band structure (and band gap), which is shown in Fig. 12. The calculated band gap (at Γ) was 1.88 eV, which is consistent with the experimentally determined values. The highest valence bands are contributed by N p orbitals, showing that its band gap can be fine-tuned by nitrogen doping. The lowest conduction bands correspond mostly to Nb d orbitals, which offer another avenue of band gap manipulation. Oxygen has a smaller effect on the band gap position.
Fig. 12 (left) Total and projected densities of states and (right) band structure for SrNbO2N, calculated at the HSE06 level. |
The reconstructed DLSR maps provide a wealth of new detail on the fidelity of the 3D printed photocatalyst design and its physico-chemical characteristics accounting for the varying lattice parameters and crystallite sizes of the active SrNbO2N phase throughout the monolith. The results of the XRD-CT characterisation efforts serve to guide the design and development of the novel tailor-made geometries and composition.
Hence, this work demonstrates that DIW is a viable approach for developing structured photocatalyst for water treatment. The resultant structured form of the photocatalyst offers the advantage of facile catalyst recovery (when compared to a powder suspension) by avoiding additional steps in product separation. We believe that 3D printing has the potential to revolutionise the field of catalysis and semiconductor photocatalysis by facilitating the controlled manufacture of both supports and catalysts at the micron level, allowing photocatalyst structures to be formed with tailored strength, porosity and functionality.
AIT, GH, MM and VM designed and implemented the material synthesis and 3D printing procedures. KN, MTS, SD and SK were responsible for aspects of photocatalytic testing (PL spectroscopy) and advised on the analysis of the photocatalytic properties while MH and BL performed and interpreted the theoretical calculations of the photodegradation mechanism. AV, VM, SDMJ and AMB designed the XRD-CT experiments, acquired the XRD-CT data and subsequently performed the Rietveld analysis of the data. VM, SK, AV, GH and BL directed the research. MTS, SD, MH, AV, AIT, GH, SK and VM are responsible for writing and editing the manuscript with feedback given by all authors.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ma01076c |
This journal is © The Royal Society of Chemistry 2023 |