Open Access Article
Wenhao Liuab,
Zhenhua Xiec,
Lihua Zhanga,
Jingguang G. Chen
*cd,
Fang Lu
*a and
Yugang Zhang
*a
aCenter for Functional Nanomaterials, Energy & Photon Sciences Directorate, Brookhaven National Laboratory, Upton, NY 11973, USA. E-mail: flu@bnl.gov; yuzhang@bnl.gov
bDepartment of Materials Science and Chemical Engineering, Stony Brook University, Stony Brook, New York 11794, USA
cChemistry Division, Brookhaven National Laboratory, Upton, New York 11973, USA
dDepartment of Chemical Engineering, Columbia University, New York, New York 10027, USA. E-mail: jgchen@columbia.edu
First published on 6th February 2026
Maximizing iridium utilization while maintaining high oxygen evolution reaction (OER) performance remains a persistent challenge in acidic water electrolysis. Immobilizing Ir on conductive, acid-stable supports is promising, yet simultaneously achieving sub-nanometer size, high area coverage, and strong electronic coupling is difficult. Here, we report a sequential surface synthesis on titanium nitride (TiN) that yields uniformly distributed sub-nanometer Ir arrays (∼0.7 nm). Our method uses ethylenediaminetetraacetic acid (EDTA) as a temporal scaffold: it chemisorbs to TiN to install dense chelating sites, captures Ir3+ ions, and confines Ir cluster growth. A subsequent thermal treatment at 500 °C in a reducing atmosphere removes the ligand shell, while preserving ultrasmall particle size and establishing direct Ir–TiN electronic coupling. The optimized catalyst exhibits mixed Ir0/Irx+ coordination with low charge-transfer resistance (Rct = 19.2 Ω), delivering a mass activity of 342 A gIr−1 at 1.54 V in acidic electrolyte. In situ X-ray absorption spectroscopy reveals irreversible surface oxidation as the primary stability-limiting factor. This stepwise strategy provides a general framework for supported catalysts that maximize precious metal utilization via sub-nanometer dispersion.
In practical proton exchange membrane water electrolyzers (PEMWEs), the anode operates in strongly acidic environments and at high current densities, which amplifies both kinetic and durability demands on the anode catalyst. Recent PEMWE studies therefore focus on reducing Ir loading while maintaining high utilization through nanoscale dispersion and conductive, corrosion-resistant supports.12 Our work addresses this design direction by enabling near-monolayer, sub-nanometer Ir dispersion on a conductive metal nitride support as a platform for acidic OER evaluation in half-cell measurements. Critically, particle size governs atomic utilization: shrinking into the sub-nanometer regime (∼0.7 nm) renders ≈90% of atoms surface-accessible to the electrolyte, versus <30% at 3 nm. However, such ultrasmall clusters cannot exist as stable free-standing entities, and they spontaneously aggregate to minimize surface energy. Strong ligands can stabilize sub-nanometer particles in solution, but these stabilized colloids are difficult to separate from solution and deposit onto electrode supports while maintaining dispersion. Even if sub-nanometer clusters could be deposited, they would rapidly migrate and coalesce under harsh OER conditions (low pH and high anodic potential). This necessitates immobilizing Ir on a conductive, acid-stable support that provides anchoring sites to prevent particle migration while facilitating charge transfer. In addition to providing mechanical and chemical stability under harsh OER conditions, the ideal supported catalyst architecture must satisfy three requirements simultaneously: (i) sub-nanometer Ir particle size to maximize surface exposure,13 (ii) near-monolayer coverage with uniform distribution to fully exploit the support surface,14,15 and (iii) intimate Ir–support contact with low-resistance electronic coupling to enable efficient charge transfer.16–19
Titanium nitride (TiN) is a promising support due to its metallic conductivity and acid stability arising from oxidation resistance.20 However, achieving the ideal Ir architecture on TiN remains challenging. The Adams fusion method, commonly used for supported Ir oxides, provides intimate metal–support contact but typically yields particles > 5 nm due to uncontrolled growth at temperatures > 500 °C. Recent colloidal approaches using poly(amidoamine) dendrimers or cetyltrimethylammonium bromide (CTAB) have reduced particle sizes to 2–5 nm IrOx on TiN,21 but this still exceeds the sub-nanometer target required for maximum utilization. Moreover, the inertness of TiN often necessitates harsh pre-activation (e.g., hydroxylation) that partially oxidizes the surface, compromising conductivity. Most critically, all current methods face a persistent challenge: strong ligands that enable sub-nanometer particle formation simultaneously prevent high-density surface attachment and create insulating barriers that block charge transfer, while weak or absent ligands allow surface contact but cause aggregation. This paradox arises because conventional one-pot approaches attempt to control particle size and surface anchoring simultaneously, inevitably forcing compromises on both.
Resolving this problem requires a multifunctional additive that (i) activates the support surface, (ii) captures metal ions, and (iii) confines cluster growth, and, crucially, deploys these functions sequentially to decouple competing processes. Ethylenediaminetetraacetic acid (EDTA), a hexadentate chelating agent, is well suited for these roles. First, EDTA can chemisorb to undercoordinated Ti sites on TiN, installing a high density of anchoring motifs across the support. Second, these surface-bound chelating groups remain available to capture Ir3+ from solution. Third, EDTA's cage-like coordination provides steric barriers that restrict particle coalescence, enabling sub-nanometer cluster formation. When these three functions operate simultaneously in conventional one-pot synthesis, stable Ir–EDTA complexes form in solution and resist surface deposition, resulting in poor coverage and ligand-blocked interfaces. However, exploiting these functionalities in a deliberate sequence can circumvent the size-versus-attachment limitation.
Here, we demonstrate a sequential surface synthesis strategy that decouples these competing requirements through four stages: (i) pre-functionalize TiN with EDTA to create high-density chelation sites, (ii) capture Ir3+ at these pre-installed anchor sites, (iii) reduce in situ to form sub-nanometer Ir while maintaining spatial confinement, and (iv) thermally remove organic residues without inducing sintering. This anchor-before-loading, then clean-after-formation workflow enables independent optimization of each step, in contrast to conventional one-pot syntheses where all processes compete simultaneously.
This methodology produces ∼0.7 nm Ir arrays with near-monolayer coverage on TiN supports. Thermal activation at 500 °C in a melamine/N2 atmosphere removes EDTA residues while preserving the sub-nanometer architecture, yielding a catalyst with coexisting Ir–O and Ir–Ir bonds. The resulting Ir@TiN-500 catalyst exhibits a mass activity of 342 A gIr−1 at 1.54 V vs. RHE, outperforming commercial IrO2. In situ X-ray absorption spectroscopy (XAS) results reveal potential-induced Ir oxidation with limited reversibility, explaining the observed stability limitation. This work establishes sequential surface synthesis as a methodology for creating well-defined supported metal catalysts, with potential applicability beyond the Ir/TiN system demonstrated here.
Catalyst inks were prepared by dispersing 3.96 mg of catalyst in a mixture of 75 µL ethanol, 25 µL isopropyl alcohol, and 3 µL Nafion D521 solution, followed by ultrasonication. The ink was drop-cast onto the GCE to achieve an Ir mass loading of 20 µgIr cm−2. Linear sweep voltammetry (LSV) curves were recorded at 20 mV s−1 with 85% iR compensation after cyclic voltammograms stabilized. All potentials were converted to the reversible hydrogen electrode (RHE) scale using E(RHE) = E(Ag/AgCl) + 0.197 V + 0.059 × pH. Electrochemical impedance spectroscopy (EIS) was performed at open-circuit potential over a frequency range of 100 kHz to 0.1 Hz with an AC amplitude of 10 mV. Chronopotentiometry stability tests were conducted at a constant current density of 10 mA cm−2 for up to 10 hours.
Our sequential strategy (Fig. 1b) resolves this by temporally separating EDTA functions rather than exploiting them simultaneously. The key insight is spatial pre-organization: by first installing EDTA as a surface-bound template on TiN before introducing the Ir precursor, we reverse the thermodynamic preference from solution-phase complexation to surface-directed coordination. In step 1, acid-treated TiN is functionalized with EDTA in the absence of Ir, allowing the chelating agent to chemisorb to undercoordinated surface Ti sites through its carboxylate groups. After washing to remove unbound EDTA, the support surface is decorated with a high-density array of anchored chelation sites with their metal-binding amine groups oriented outward. In step 2, Ir3+ is introduced. Since no excess EDTA remains in solution, Ir3+ coordinates exclusively to these immobilized sites rather than forming free solution complexes. This spatial confinement is critical: because each Ir center is pre-anchored to a specific surface location, subsequent reduction becomes a heterogeneous surface-confined process rather than homogeneous solution-phase nucleation. In step 3, addition of NaBH4 reduces Ir3+ to metallic Ir0. The surface-bound EDTA scaffold maintains spatial isolation between adjacent nucleation sites, preventing migration and coalescence during reduction, enabling the formation of sub-nanometer clusters in intimate contact with the underlying TiN support. However, the as-synthesized material retains residual EDTA coordination that electronically isolates Ir from TiN. Step 4 addresses this through controlled thermal treatment in a reducing atmosphere (melamine/N2), thermally decomposing the organic EDTA residues. Critically, the Ir–TiN interaction established during surface-directed reduction (step 3) is sufficiently strong to prevent sintering during organic removal, preserving the sub-nanometer architecture while simultaneously cleaning the interface to enable direct electronic coupling.
This sequential workflow converts an unfavorable process (depositing kinetically stable Ir–EDTA complexes onto inert TiN) into a favorable one (capturing Ir3+ at pre-installed, surface-bound chelation sites). Each stage addresses a specific requirement: EDTA anchoring enables high-density coverage (requirement (ii)), surface-confined Ir3+ capture followed by reduction achieves sub-nanometer size (requirement (i)), and thermal activation establishes direct contact between Ir and TiN (requirement (iii)). Unlike one-pot synthesis, where all processes compete, the sequential approach allows independent optimization of each step.
CTAC-mediated synthesis (Fig. 2b) provides moderate improvement, yielding primary particles with a mean diameter of 1.6 ± 0.3 nm (Fig. 2e). However, these particles form agglomerations of ∼100 nm on the TiN surface, achieving only 41% surface coverage (Fig. 2f). The distribution remains heterogeneous with clearly visible uncoated areas. The one-pot EDTA co-deposition approach (Fig. 2c) produces sub-nanometer primary particles with a size of 0.8 ± 0.2 nm, substantially smaller than both the no-ligand and CTAC cases. However, it only achieves ∼48% surface coverage (Fig. 2f), which still leaves many bare regions. This confirms the challenge outlined in Section 2.1: kinetically stable solution-phase Ir–EDTA complexes that enable size control simultaneously resist adsorption on the TiN surface.
In contrast, the sequential EDTA pre-anchoring approach (Fig. 2d) produces uniform sub-nanometer particles with a mean diameter of 0.70 ± 0.16 nm (Fig. 2e) that densely decorate the TiN surface with ∼96% coverage (Fig. 2f), which is more than a tenfold improvement over the no-ligand control and more than a fourfold improvement over one-pot EDTA. No large aggregates or bare regions are observed across multiple imaging areas. The narrow size distribution indicates uniform nucleation kinetics consistent with templated growth at pre-defined surface sites. To clarify the support role of TiN, we prepared a control sample without TiN, in which the Ir precursor was reduced in the presence of EDTA in solution (denoted as Ir/EDTA, no TiN; Fig. 2e and S3). TEM shows that EDTA can temporarily stabilize ultrasmall Ir clusters (∼0.78 nm). However, this dispersion remains ligand-capped, which is expected to partially block surface sites and hinder electron transfer to the electrode substrate during electrochemical testing. Attempts to remove EDTA without a solid anchoring surface lead to aggregation, so this TiN-free sample serves as a structural control rather than an electrochemical benchmark for metal–support coupling. This underscores the essential role of TiN anchoring in enabling ligand removal while preserving sub-nanometer dispersion.
The performance scoring matrix (Fig. 2g) quantifies these observations against the three criteria: sub-nanometer size, high coverage, and unobstructed contact. The no-ligand method provides contact but fails on size and coverage. CTAC achieves partial scores on all metrics but excels at none. One-pot EDTA succeeds on size but fails on coverage and electronic contact due to residual ligand shells. Only sequential synthesis satisfies all requirements simultaneously.
To address this insulating barrier while preserving the sub-nanometer architecture, we performed a systematic thermal treatment study at 400, 500, 600, 700, and 800 °C under a melamine/N2 atmosphere. Melamine serves as a nitrogen-rich reducing agent that decomposes at elevated temperatures to generate NH3 and other reducing species, preventing TiN oxidation while facilitating organic decomposition. This optimization study (detailed in Section 3.4) identifies 500 °C as the optimal condition, achieving EDTA removal without inducing sintering. Fig. 3 presents structural characterization of the optimized Ir@TiN-500 catalyst.
Transmission electron microscopy reveals uniform Ir distribution across multiple length scales (Fig. 3). Low-magnification TEM (Fig. 3a) shows multiple TiN nanoparticles uniformly decorated with sub-nanometer Ir, with no preferential deposition on specific regions or crystal facets, confirming that high-density coverage extends across the entire sample. Medium-magnification TEM (Fig. 3b) reveals a dense array of discrete Ir nanoparticles covering approximately 90% of the TiN support surface.
High-resolution TEM (Fig. 3c) shows the crystalline nature of individual Ir nanoparticles. Clear lattice fringes with a d-spacing of 0.22 nm correspond to the Ir(111) planes of face-centered cubic metallic iridium. Both Ir and TiN lattices are visible with no amorphous structure at the interface, indicating that thermal treatment has eliminated the EDTA coordination shell without triggering sintering. The particle size histogram (Fig. 3d) shows a narrow Gaussian distribution centered at 0.75 ± 0.2 nm.
High-angle annular dark-field scanning TEM (HAADF-STEM, Fig. 3e) shows bright Ir nanoparticles uniformly distributed across the darker TiN support. The particle density is comparable to the as-synthesized sequential material (Section 3.2), further confirming that thermal treatment does not cause particle migration or coalescence. Energy-dispersive X-ray spectroscopy elemental mapping (Fig. 3f) shows spatial overlap of Ir, Ti, and N signals across the mapped region, indicating uniform distribution with no phase segregation or Ir-rich domains. The homogeneous Ir signal across multiple TiN grains demonstrates reproducible coating independent of local variations in support morphology.
X-ray diffraction patterns (Fig. 4c) confirm that the TiN support maintains its crystalline structure across all annealing temperatures. The characteristic cubic TiN reflections at 36.7°, 42.6°, and 61.8° corresponding to (111), (200), and (220) planes show no shift or broadening. No TiO2 peaks appear even after 800 °C treatment, demonstrating that the melamine/N2 atmosphere prevents support oxidation. For Ir, no diffraction peaks appear in samples treated at ≤600 °C despite ∼10 wt% loading, consistent with highly dispersed/sub-nanometer clusters below XRD detection. A weak Ir(111) reflection emerges only at 700 °C and becomes more pronounced at 800 °C, indicating coalescence into large particles, in agreement with TEM-observed sintering.
XPS analysis of the N 1s region (Fig. 4e) tracks EDTA decomposition. The as-synthesized material shows a strong peak at 396.5 eV assigned to amine nitrogen coordinated to Ir3+ in the Ir–EDTA complex and a weak peak at 399.6 eV from N–C bonds in EDTA. At 400 °C, the peak at 399.6 eV shifts to ∼398.9 eV and increases dramatically in intensity, indicating nitrogen dissociation from Ir centers and migration toward the TiN support as EDTA fragments. By 500 °C, the EDTA-derived nitrogen signal at 399.6 eV is essentially eliminated. At 700–800 °C, the spectrum is dominated by the Ti–N nitrogen peak at 396.4 eV, indistinguishable from the pristine support, confirming complete organic removal. Ti 2p XPS shows minimal changes across all temperatures, with peaks at ∼463.4 eV and 457.7 eV remaining stable, indicating persistent Ti–N bonding. Together, these results confirm that the melamine-generated reducing atmosphere suppresses bulk TiN oxidation to insulating TiO2 and preserves support conductivity.
219.8 eV (as-synthesized, near IrO2 at 11
220.0 eV) to 11
218.2 eV (800 °C, approaching Ir foil at 11
217.9 eV). The 500 °C sample occupies an intermediate position at 11
218.9 eV, confirming the presence of mixed Ir0/Irx+ species identified by XPS.
Extended X-ray absorption fine structure (EXAFS) analysis (Fig. 5c) reveals local coordination environment. The Fourier-transformed EXAFS spectra show two coordination shells: Ir–O/N at ∼1.6 Å (phase-uncorrected) and Ir–Ir metallic bonds at ∼2.7 Å. The as-synthesized material exhibits a dominant Ir–O peak with negligible Ir–Ir intensity, confirming isolated Ir atoms or very small clusters encapsulated by EDTA. At 400 °C, the Ir–O peak decreases while a small Ir–Ir peak emerges, indicating partial decomposition of the ligand shell and densification of Ir within still-confined, sub-nanometer clusters anchored at the original sites, rather than coalescence or the formation of bulk-like metallic bonding. By 500 °C, Ir–O and Ir–Ir intensities are comparable, reflecting small Ir0 cores with mixture-coordinated surface species (Ir–O/Irx+) while the clusters remain sub-nm and spatially pinned. At 600–800 °C, the Ir–Ir peak becomes strongly dominant, and Ir–O nearly vanishes, indicating growth into bulk-like metallic nanoparticles.
Quantitative coordination number (CN) analysis from EXAFS fitting (Fig. 5d) shows a progressive transition with increasing temperature. The as-synthesized material shows CN(Ir–O) = 6.3 ± 0.8 and CN(Ir–Ir) = 0.2 ± 0.2, consistent with isolated Ir centers surrounded by EDTA. At 500 °C, CN(Ir–O) = 2.3 ± 0.3 and CN(Ir–Ir) = 5.3 ± 0.5, representing the crossover point. By 800 °C, CN(Ir–O) drops to 0.8 ± 0.2, while CN(Ir–Ir) reaches 8.8 ± 1.1, approaching bulk metallic coordination (CN = 12 for fcc Ir). The Ir–Ir CN of 5.3 at 500 °C is consistent with a cuboctahedral 13-atom cluster (∼0.75 nm diameter), which would have an average CN of ∼5.5 for interior atoms. This agreement between EXAFS-derived coordination and TEM-measured size validates both techniques. In contrast, the 800 °C CN of 8.8 indicates particles approaching 2–4 nm with bulk-like coordination.
Wavelet transform (WT) analysis (Fig. 5e) provides enhanced k–R space resolution, separating light-atom (O, N) from heavy-atom (Ir) backscattering. The as-synthesized material (Fig. 5e) shows intensity concentrated at low k-values (2–6 Å−1) and R ∼ 1.6 Å, the signature of Ir–O/N coordination from EDTA. Ir@TiN-500 exhibits a bimodal pattern with intensity at both low R/distributed k (Ir–O contribution) and high R/high k (R ∼ 2.7 Å, k > 7 Å−1, Ir–Ir metallic scattering). This k–R fingerprint confirms the coexistence of two distinct coordination environments. Ir@TiN-800 shows predominantly high-R, high-k intensity, characteristic of extended Ir–Ir coordination in metallic Ir clusters.
The convergence of multiple characterization techniques establishes 500 °C as the optimal processing temperature. Below 500 °C, incomplete EDTA removal leaves organic barriers despite favorable particle size. Above 500 °C, complete organic elimination is achieved, but thermal energy triggers sintering. At 500 °C, three conditions coincide: (1) TEM and XRD confirm sub-nanometer size retention (0.75 nm) with crystallization, (2) XPS demonstrates complete EDTA removal, and (3) XAS reveals a mixed Ir0/Irx+ electronic state with both Ir–Ir and Ir–O coordinations. We interpret this mixed Ir0/Irx+ signature as an activity–stability trade-off: the coexistence of metallic domains (promoting conductivity) with surface oxide species (providing OER-active sites) enhances initial atomic utilization and kinetics, while under prolonged OER bias this mixed state can evolve irreversibly toward more oxygenated/disordered local structures, compromising long-term durability as revealed by in situ XAS in Section 3.6.
Electrochemical surface area (ECSA) estimated from double-layer capacitance (Cdl) measurements (Fig. 6e) shows that Ir@TiN-500 exhibits the largest capacitance (6.16 mF cm−2), confirming high accessibility of Ir surface atoms. This reflects the sub-nanometer particle size (0.9 nm) maintained after thermal treatment, where approximately 90% of atoms remain surface-exposed. Samples annealed at 700–800 °C show progressively lower Cdl (4.2 and 3.1 mF cm−2, respectively) consistent with particle growth. The as-synthesized and 400 °C samples also exhibit low Cdl (2.8 and 3.4 mF cm−2, respectively) despite favorable size, suggesting that residual EDTA physically blocks electrolyte access. ECSA-derived normalization is provided in Fig. S21b as a comparative metric, while noting that double-layer capacitance can be influenced by surface chemistry and wettability across ligand/annealing treatments. Ir@TiN-500 exhibits much higher ECSA-normalized activity than commercial IrO2 after complete organic removal. At the same Ir loading, it also delivers the highest TOF, consistent with maximized site accessibility (Fig. S21a). Electrochemical impedance spectroscopy (EIS, Fig. 6d) quantifies interfacial charge-transfer resistance (Rct). We note that EDTA pre-functionalization introduces an organic interlayer prior to annealing, which can transiently increase interfacial resistance in the as-prepared and low-temperature samples. After annealing, progressive ligand removal reduces this barrier and enables more direct electronic contact between Ir and TiN. Consistent with this interpretation, Ir@TiN-500 achieves the lowest Rct of 19.2 Ω, indicating efficient charge transfer between Ir and TiN after EDTA removal, whereas the as-synthesized (Rct > 380 Ω) and 400 °C (Rct > 4300 Ω) samples exhibit high resistance, likely due to ligand-derived blocking and incomplete/heterogeneous interfacial cleaning (Table S1). At higher temperatures, Rct increases again (51.7 Ω at 800 °C) despite complete organic removal and full Ir reduction to a metallic state, consistent with Ir coarsening that reduces the total Ir–TiN interfacial contact area per geometric electrode area. Notably, the fitted series resistance (Rs) varies only modestly across the thermal treatment using the same TiN support, whereas Rct changes by orders of magnitude and tracks with ligand removal and interfacial contact evolution. This comparison confirms that the dominant differences arise from interfacial charge transfer rather than bulk support conductivity changes. Chronopotentiometric stability testing at 10 mA cm−2 shows that Ir@TiN-500 maintains stable potential for approximately 9.5 hours, the longest among the series, though still limited compared to state-of-the-art stable OER catalysts. This observation motivates the in situ XAS investigation (Section 3.6), which reveals that electronic/chemical transformation rather than sintering limits durability.
Fig. 6c summarizes the key performance metrics of catalysts treated at different temperatures. The volcano-shaped activity trend identifies 500 °C as optimal, with mass activity peaking sharply while overpotential reaches its minimum. This optimization reflects the balance between EDTA removal and size preservation: below 500 °C, EDTA blocks performance despite ideal size; above 500 °C, sintering reduces active site density despite clean interfaces. The correlation between structures featuring sub-nanometer size, mixed Ir0/Irx+, and low Rct and performance with high activity and large ECSA validates the advantage of the sequential synthesis design strategy. Representative literature benchmarks for acidic OER Ir-based catalysts (activity metrics, durability metrics, and test conditions) are summarized in Table S11; comparisons should be interpreted by taking into consideration differences in loading, electrolyte, iR correction, and metric definitions across reported literature. Within these constraints, the higher mass activity observed here is consistent with the high Ir utilization enabled by sub-nanometer Ir dispersion and efficient electronic contact with the conductive TiN support.
In situ XANES spectra for Ir@TiN-500 (Fig. 7a) show systematic evolution as potential increases from open-circuit (0.4 V) through the OER regime (1.32–1.65 V vs. RHE). The white-line intensity progressively increases and shifts to higher energy with applied potential, indicating oxidation of Ir (Ir0 → Irx+ → Ir4+). The initial state at 0.4 V shows lower white-line intensity than commercial IrO2, consistent with the mixed Ir0/Irx+ character established in Section 2.4. As the potential increases to 1.65 V, the white-line approaches but does not reach the IrO2 reference, suggesting partial surface oxidation rather than complete conversion to bulk oxide.
When potential is returned to 0.4 V after the OER scan, the white-line intensity does not fully recover to its initial state, revealing hysteresis indicative of irreversible oxidation. Quantitative analysis of the white-line position (Fig. 7c) shows that the centroid energy increases from 11
217.9 eV (initial 0.4 V) to 11
219.1 eV (1.65 V) and then decreases to only 11
218.1 eV upon return, leaving a residual shift of 0.3 eV. Similarly, integrated white-line intensity (Fig. 7c) increases from 2.0 to 2.6 a.u. during the forward scan but recovers to only 2.5 a.u. on the return. This persistent elevation indicates that a substantial fraction of Ir sites oxidized during the OER remain in higher oxidation states even after removing the driving potential. For comparison, in situ XANES of the as-synthesized Ir@TiN (Fig. 7b) shows different behavior. The initial white-line intensity is higher than that of Ir@TiN-500, reflecting the predominantly Ir4+ character from EDTA coordination. During the OER scan, the white-line changes less dramatically than Ir@TiN-500 and shows limited reversibility upon return. At all potentials, Ir@TiN-500 maintains lower white-line energy and intensity than the as-synthesized material before OER cycling, indicating more metallic character.
In situ Fourier-transformed EXAFS spectra (Fig. 7e) provide atomistic evidence for the oxidation process. At the initial 0.4 V state, Ir@TiN-500 shows the bimodal pattern established in Section 3.4: peaks at both ∼1.9 Å (Ir–O) and ∼2.7 Å (Ir–Ir). As potential increases to OER conditions, the Ir–O peak grows substantially while the Ir–Ir peak systematically weakens, consistent with oxidative conversion of metallic Ir–Ir bonds to Ir–O bonds. Upon returning to 0.4 V, the coordination environment shows limited recovery. The Ir–O peak remains elevated compared to the initial state, while the Ir–Ir peak fails to return to its original intensity. Quantitative coordination number analysis (Fig. 7f) shows that CN(Ir–Ir) decreases from 4.6 ± 0.5 (initial 0.4 V) to 0.7 ± 0.5 (1.54 V), representing a substantial loss of metallic bonds. Upon return to 0.4 V, CN(Ir–Ir) recovers to only 0.3 ± 0.9, indicating limited reversibility. Complementarily, CN(Ir–O) increases from 2.4 ± 0.3 (initial) to 5.9 ± 0.5 (1.65 V) and then decreases to 5.2 ± 1.2 upon return, remaining elevated above the initial value. These changes suggest substantial oxidative restructuring of the catalyst surface under OER conditions. Wavelet transform (WT) analysis shown in Fig. 7g also confirms the transformation of Ir–Ir to Ir–O during the OER process. The as-synthesized Ir@TiN shows different behavior under OER conditions (Fig. S18 and Table S10). Starting with predominantly Ir–O coordination (CN ∼ 6.4, minimal Ir–Ir), it undergoes limited further changes during the potential cycle, consistent with already being in a stable oxidized state.
The in situ XAS results explain the ∼9.5 hour OER stability limitation observed in Section 3.5. The irreversible oxidation revealed by XANES hysteresis and incomplete EXAFS coordination recovery indicates substantial restructuring of the ultrasmall Ir domains under OER conditions. Importantly, a decrease in the Ir–Ir EXAFS contribution can arise from multiple concurrent effects, including partial oxidation toward an IrOx-like local structure, increased static/dynamic disorder, and fragmentation/restructuring that lowers the average metallic coordination number even if the total Ir loading remains similar. These trends are consistent with mechanistic understanding linking OER-driven restructuring (including lattice-oxygen processes) with Ir instability in acid;23 however, Ir dissolution is not quantified in this work and cannot be concluded from in situ EXAFS alone. In addition, oxygen incorporation at the Ir–TiN interface may weaken metal–support interactions, as the formation of interfacial Ti–O–Ir bonding could disrupt the facile charge transfer established by thermal treatment. Overall, the mixed Ir0/Irx+ signature at 500 °C reflects an activity–stability trade-off: intimate contact with conductive TiN promotes high initial kinetics, while in situ XAS indicates irreversible oxidation/reconstruction toward more oxygenated/disordered motifs under acidic OER conditions, consistent with the observed stability limitation.
Multi-parameter correlation analysis (Fig. 8b) demonstrates that mass activity correlates positively with Cdl (R2 = 0.82) and CN(Ir–Ir) up to ∼5 and inversely with Rct (R2 = 0.89) and particle size beyond 1 nm (R2 = 0.78). These quantitative relationships confirm that the three requirements (sub-nanometer size, high coverage, and charge transfer between Ir and TiN) directly govern performance. The radar plot (Fig. 8c) integrating eight normalized metrics shows that Ir@TiN-500 exhibits a balanced profile across activity, kinetics, surface area, resistance, size, coordination, and stability. The correlation heatmap (Fig. 8d) confirms that activity strongly correlates with electronic (1/Rct) and structural (Cdl, size) descriptors, while stability correlates weakly with initial performance metrics, indicating that degradation involves chemical/electronic transformation of Ir rather than structural coarsening.
The integrated characterization reveals that activity maximization and stability represent distinct challenges requiring different strategies. The optimization of treatment temperature successfully balances organic removal with size preservation, creating a mixed Ir0/Irx+ coordination environment that combines high conductivity with OER activity. Quantitative structure–performance correlations establish clear design criteria for enhanced activity, which is enabled by sub-nanometer size, balanced metallic/oxidic character, and low interfacial resistance. However, in situ spectroscopic measurements reveal severe structural transformation: the high surface atom fraction that enables superior activity creates extreme vulnerability under harsh operating conditions. The mixed Ir0/Irx+ state undergoes oxidation during the OER, with loss of a large portion of metallic Ir–Ir bonds. This demonstrates that while sequential synthesis establishes stronger metal–support interactions than conventional methods, it cannot prevent fundamental structural transformation of the highly reactive sub-nanometer clusters. Future strategies to address this limitation could include: (1) controlled pre-oxidation to convert metallic Ir0 to IrOx species, establishing a more fully oxidized/oxygenated local structure. We note that while such oxidized structures are often associated with improved initial OER kinetics, they have also been linked in the literature to Ir instability pathways under acidic OER conditions, representing a complex optimization challenge. (2) Interface engineering to create stronger Ir–TiN bonding that prevents oxygen insertion at the interface, such as through controlled nitridation or introduction of interfacial buffer layers that maintain charge transfer while blocking interfacial oxidation. The characterization framework combining ex situ multi-technique analysis with in situ measurements provides a methodology for evaluating these strategies and understanding degradation mechanisms in other supported catalyst systems. We note that translation from half-cell measurements to PEMWE-relevant current densities will additionally require catalyst-layer optimization, including higher Ir area loading and transport-engineered architectures to address mass transport limitations at high current densities. Such catalyst-layer engineering is beyond the scope of the present RDE-type evaluation but represents an important direction for future work toward practical device integration.
| This journal is © The Royal Society of Chemistry 2026 |