Bharti Rani
,
Jitendra Kumar Yadav
,
Priyanka Saini
,
Anant Prakash Pandey
and
Ambesh Dixit
*
Advanced Material and Devices Laboratory (A-MAD), Department of Physics, Indian Institute of Technology, Jodhpur, Rajasthan 342030, India. E-mail: ambesh@iitj.ac.in
First published on 3rd June 2024
Owing to their attractive energy density of about 8.1 kW h kg−1 and specific capacity of about 2.9 A h g−1, aluminum–air (Al–air) batteries have become the focus of research. Al–air batteries offer significant advantages in terms of high energy and power density, which can be applied in electric vehicles; however, there are limitations in their design and aluminum corrosion is a main bottleneck. Herein, we aim to provide a detailed overview of Al–air batteries and their reaction mechanism and electrochemical characteristics. This review emphasizes each component/sub-component including the anode, electrolyte, and air cathode together with strategies to modify the electrolyte, air-cathode, and even anode for enhanced performance. The latest advancements focusing on the specific design of Al–air batteries and their rechargeability characteristics are discussed. Finally, the constraints and prospects of their use in mobility applications are also covered in depth. Thus, the present review may pave the way for researchers and developers working in energy storage solutions to look beyond lithium/sodium ion-based storage solutions.
More interestingly, due to the high theoretical capacity and energy density of metal–air batteries, they have shown potential as alternatives to the currently dominating Li-ion batteries. Furthermore, the weight of metal–air batteries is also one of the exciting factors given that oxygen from air acts as the cathode material. Thus, in principle, this reduces the need for a cathode in these energy storage systems.26–28 Generally, these batteries are equipped with metal as the anode and an air-penetrating current collector to complete the circuit.29,30 The battery is vitalized with a suitable electrolyte between the metal and current collector to provide a medium for efficient ionic conduction. Presently, various metal–air batteries are the subject of research, aiming to find better alternatives to the existing Li-ion energy storage solutions.31–33 Firstly, lithium has the highest theoretical energy density compared to conventional batteries, i.e. the lithium–air (Li–air) battery has an energy density of 13000 W h kg−1 but suffers from numerous challenges despite being rechargeable, unlike other air batteries. Furthermore, the operation of Li–air batteries is not convenient in a humid environment, which makes them unstable. Another challenge is the blockage of their porous current collector from residue. Moreover, there is still a lack of understanding of how catalysts work in the rechargeability of Li–air batteries. The penetration of CO2 leads to the formation of alkali carbonate residues, which is another complex issue that needs to be addressed with these energy storage systems.34–37 However, Li–air batteries have a significantly higher energy density than their lithium-ion counterparts, translating to a longer range for electric vehicles and extended runtime for electronics. Nevertheless, the associated challenges remain the same, thus limiting their commercial use to date. These batteries utilize reactive lithium metal anodes and require open designs for air intake, raising safety concerns. Additionally, issues related to the electrolyte stability, cathode clogging, and overall cycle life hinder their practical use. In this scenario, switching from Li–air batteries is crucial for sustainable future energy technology.29,38–41
Another metal–air battery that has emerged as an attractive alternative is the zinc–air battery due to its non-toxic nature and ease-of-fabrication under normal conditions. However, it is also associated with some challenges, such as dendrite formation in the zinc anode during multiple charge–discharge cycles, non-uniform dissolution due to precipitation of zinc residue, limited solubility of oxygen, and high overpotential.42–47 Similarly, Fe–air batteries have also been explored due to their many advantages, including the abundance of iron and low cost, making them potentially cost-effective for large-scale energy storage applications. However, Fe–air batteries face certain challenges such as limited rechargeability, low efficiency due to the sluggish oxygen reduction kinetics, and issues related to iron anode degradation and electrolyte management.48–50
Recently, Al–air batteries have been widely explored due to the enormous advantage of the aluminum metal anode. Firstly, aluminum is one of the most abundant elements in the Earth's crust, making it an attractive and sustainable choice for large-scale energy storage applications.51–54 Secondly, aluminum has a higher energy density than zinc and iron, potentially surpassing existing metal–air batteries in specific energy and power (comparison of different metal anodes and metal–air batteries shown in Fig. 1 and Table 1, respectively). These attractive features make Al–air batteries promising for application in electric vehicles, grid-scale energy storage, and other critical areas due to their high energy density, potential for longer battery life, and environmental advantages over existing technologies. Thus, due to their potential as an alternative to existing battery technologies, Al–air batteries are the primary focus of this review.55,56 Additionally, Al–air batteries have the potential to be more environmentally friendly, given that aluminum is readily recyclable and poses fewer environmental concerns compared to other metals.57,58
Fig. 1 A comparison of the gravimetric and volumetric capacity, Earth-crust abundance and cost of metal-anodes. |
S. N. | Battery system | Redox reaction | Battery type | Theoretical OCP (V) | Practical OCP (V) | Theoretical specific energy (W h kg−1) | Ref. |
---|---|---|---|---|---|---|---|
1 | Li–air | 2Li + O2 ↔ Li2O2 | Secondary | 2.96 | 2.4–2.8 | 3500 | 59 |
2 | Na–air | Na + O2 ↔ NaO2 | Secondary | 2.27 | 2.2–2.3 | 1108 | 60 |
3 | Al–air | 4Al + 3O2 + 6H2O → 4Al(OH)3 | Primary | 2.71 | 1.2–1.6 | 2784 | 61 and 62 |
4 | Mg–air | 2Mg + O2 + H2O → 2Mg(OH)2 | Primary | 2.77 | 1.2–1.4 | 2848 | 61 and 63 |
5 | Zn–air | 2Zn + O2 ↔ 2ZnO | Secondary | 1.65 | 1–1.2 | 1086 | 63 and 64 |
6 | Fe–air | 3Fe + 4O2 ↔ Fe3O4 | Secondary | 1.28 | 0.6–1.0 | 764 | 65 |
Aluminum-based batteries have undergone significant development since their inception, with notable milestones including the introduction of Al–MnO2 batteries around the 1960s and subsequent efforts to improve their efficiency and applicability. Initially, Al was employed as an anode in the Buff cell in conjunction with a carbon cathode around 1857, then went on a long journey to the current form of Al-based energy storage systems, further explored based on Al–MnO2 batteries, and later extended by Zaromb et al. to Al–O2 batteries.66 The development over time is schematically summarized in Fig. 2(a).67 To date, continuous efforts have been devoted to processing Al–O2 batteries under ambient conditions, where ambient O2 can be utilized as an efficient cathode in these systems. Recently, Al–air batteries have attracted attention for their use in strategic fields, i.e., marine and military applications, because of their high energy density. Given that their working mechanism is somewhat comparable to that of fuel cells, researchers have also started looking into that direction as well.68,69 Nowadays, companies such as Phinergy and Alcoa are devoting their efforts to employing Al–air batteries for e-vehicles.70,71 However, despite the reported advances, there are various constraints associated with these batteries, which should be addressed to make Al–air batteries fully-efficient for large-scale systems and mobility applications.72–74
Fig. 2 (a) Timeline of aluminum-based batteries explaining the development of Al–air batteries with time. (b) Publication trend with the year for Al–air battery (source: https://www.webofscience.com/).75 |
The Al–air battery has been the subject of intense research for the past few decades, as has been observed from previous discussions related to its journey and timeline. Fig. 2(b) illustrates the publication trend and timeline of aluminum-based batteries sourced from the Web of Science database.75 However, its associated issues such as corrosion, non-reversible reactions, stability, and self-discharge in a non-use state still prevent its successful transition from the laboratory to end-use. Aluminum corrosion in aqueous electrolytes is the biggest barrier in the application of the Al–air battery, which needs to be managed effectively for its potential use. The Al–air battery tends to form a passive oxide layer as a result of corrosion in the aqueous electrolyte, which is the main reason for its limited effective use even after various attempts have been made since Zaromb's research (i.e. from the early 60's) to date.66,76–80 Therefore, various methodologies have been introduced in the literature to minimize its corrosion such as alloying of Al, surface coatings, introducing an additive in the electrolyte, and using water-in-salt and non-aqueous, such as different electrolyte media. Thus, this review provides a comprehensive analysis, including the underlying functioning mechanism and electrochemical interactions, to mitigate some of these issues. A thorough and detailed review is presented, emphasizing the current status of each constituent of the Al–air battery, including its anode, electrolyte, and catalyst. In addition, the potential rechargeability of Al–air batteries is also highlighted together with their geometrical structures/designs for efficient performances. The focus is the current prevailing obstacles and future prospects for Al–air batteries.
Al-characteristics (parameters) | Value | Reference |
---|---|---|
Abundance (wt%) | 8.1 | 90 |
Melting point (°C) | 660.4 | 91 |
Atomic radius (Å) | 1.431 | 48 |
Ionic radius (Å) | 0.53 | 92 |
Covalent radius (Å) | 1.25 | 93 |
E° vs. SHE (V) | −1.66 | 91 |
HER onset potential vs. SHE (V) | −0.47 | 91 |
Bond dissociation energy Al–O (kJ mol−1) | 512 | 82 |
Bond dissociation energy Al–Al (kJ mol−1) | 186 | 82 |
Al–H bond energy (kJ mol−1) | 285 | 91 |
Theoretical energy density (W h kg−1) | 8100 | 94 |
Theoretical specific capacity (mA h g−1) | 2980 | 95 |
Cost (US$ per kg) | 1.9 | 92 |
Aluminum forms a crystal in the Fmm space group, with the lattice parameter of a = 4.04 at ambient temperature and pressure.73 The inherent structural integrity of Al and its extensive crystal structures make it an attractive candidate as the negative electrode in batteries. Additionally, its ability to form intermetallic phases with a wide range of crystal structures further enhances its potential for battery applications.66,68,69,72–74,87–89
One of the primary obstacles associated with the use of aluminum as a material for active batteries pertains to its strong affinity to oxygen, resulting in the oxidation of the newly formed aluminum surface when exposed to oxygen, water, or other oxidizing agents. Under standard conditions, the enthalpy of solid oxide formation is around 1675 kJ mol−1, exceeding the enthalpy of the oxidation reaction of iron (Fe) to Fe3O4, which is around 1121 kJ mol−1, and to Fe2O3 of ∼822.2 kJ mol−1.96,97 However, aluminum can rapidly generate a thin, uniform, and continuous amorphous Al2O3 surface layer of a few nanometers, i.e., ∼2 to 10 nm thickness.87 According to Yang and team, the dielectric and amphoteric oxide layer exhibits liquid-like behavior when subjected to stress, hence demonstrating self-healing capabilities. The oxide layer exhibits compression relative to the underlying aluminum, which can withstand deformation without experiencing fracture.98 This is why it provides several advantages when used as a current collector in lithium and other batteries. The formed oxide layer does not behave as a complete dielectric, but still provides electric conduction due to the tunneling effect even after adding up the contact resistance of the order of kΩ. Conversely, it creates an obstacle for the solvation of aluminum, which presents a difficulty in utilizing aluminum metal as a negative electrode.80 Therefore, this inherent oxide impacts the electrochemical characteristics, specifically the overpotential of aluminum as an anode.99 Typically, a secondary layer is created on the oxide layer by reacting with the surrounding gases and liquids. The continuous oxide layer closest to the metal surface transforms into a hydroxylated film at the interface between the solid and gas. This becomes a barrier if the aluminum battery is intended to be electrically rechargeable.100 Ultimately, the abundance, structural integrity, and ability to form intermetallic phases of aluminum make it a compelling candidate for battery applications despite challenges such as oxidation and oxide layer formation. Accordingly, addressing these challenges is crucial for realizing the full potential of aluminum-based batteries in industrial-scale energy storage solutions including both Al-ion and Al–air batteries.
Fig. 3 Schematic representation of the working mechanism of a complete Al–air battery with the respective electrodes and overall reaction. |
Anodic half-cell reaction:
Al + 3OH− → Al(OH)3 + 3e− (−2.31 V vs. SHE) | (1) |
Cathodic half-cell reaction:
O2 + 2H2O + 4e− → 4OH− (0.40 V vs. SHE) | (2) |
Overall reaction:
4Al + 3O2 + 6H2O → 4Al(OH)3 (2.71 V vs. SHE) | (3) |
An aqueous alkaline electrolyte medium increases the likelihood of the hydrogen evolution reaction (HER), leading to the rapid depletion of the Al anode due to undesirable features.79 HER causes Coulombic loss during discharge by the evolution of hydrogen gas from the anode surface, as mentioned in eqn (4) and (5). Usually, the aluminum anode in alkali solutions faces two significant problems, besides HER. The initial stage involves the formation of a passive oxide layer, which causes a reduction in the operational cell voltage, and later increases both the mass and charge transfer resistance, decreasing the open circuit potential (OCP).111 Consequently, the realistic energy density and cell voltage are restricted. Another problem related to aluminum anodes is the rapid corrosion rate caused by removing the oxide layer. The theoretical OCP of 2.74 V has been observed practically in the range of 1.2 to 1.6 V due to corrosion and the formation of a passivating layer.74 During an open circuit, the reduction of water and the occurrence of self-corrosion can be understood with eqn (4) and (5), as follows:113
Water reduction reaction:
2H2O + 2e− → 2OH− + H2 (−0.83 V vs. SHE) | (4) |
Self-corrosion reaction:
2Al + 2H2O + 2OH− → 2Al(OH)4− + 3H2 (1.48 V vs. SHE) | (5) |
The corrosion problem was initially addressed using two approaches, as follows: (i) modification of the aluminum anode and (ii) selection of a compatible electrolyte. Anode modification was performed using either an aluminum alloy or applying a protective layer, modifying anode grain size and crystal orientation. Also, alkali electrolytes are widely explored with numerous modifications, such as adding additives, changing the medium from aqueous to ionic, forming a gel/solid electrolyte, dual electrolyte systems, and oil displacement. Each type of electrolyte has advantages and disadvantages.111,114 More details about the different types of electrolytes are discussed in the following section, as well as their impact on the overall performance and efficiency of Al–air batteries.
However, the sluggish ORR in the Al–air battery limits the potential of this battery and complicates the process.115 The intermediate steps, together with the activation of oxygen, removal of oxides, and bonding of oxygen atoms should considered to understand the complete mechanism.116
The ORR mechanism is different in acidic (eqn (6)–(8)) and alkaline media (eqn (9)–(13)), which are mentioned in the following reactions:57,102
ORR in acidic medium:
O2 + 4H+ + 4e− → 2H2O {4-electron transfer} | (6) |
O2 + 2H+ + 2e− → H2O2 {2-electron transfer} | (7) |
H2O2 + 2H+ + 2e− → 2H2O | (8) |
ORR in alkali medium (9)–(12):117
X + O2 + H2O + e− → XOOH + OH− | (9) |
XOOH + e− → XO + OH− | (10) |
XO + H2O + e− → XOH + OH− | (11) |
XOH + e− → X + OH− | (12) |
Overall reaction:
O2 + 2H2O + 4e− → 4OH− | (13) |
There is one more possibility of oxygen and the catalyst interacting for the ORR process, which occurs perpendicular to the surface. In this situation, two-electron transfer occurs during the process and hydroperoxides are evolved during the intermediate steps, as shown in the following reactions (14)–(16):57,102,117
O2 + H2O + e− → HO2,ads + OH− | (14) |
HO2,ads + e− → HO2− | (15) |
Overall reaction:
O2 + H2O + 2e− → HO2− + OH− | (16) |
After undergoing the previously indicated two-electron reaction, hydroperoxide has the potential to undergo either a further two-electron reduction or chemical disproportionation, as depicted in the following equation:74
HO2− + H2O + 2e− → 3OH− | (17) |
2HO2− → 2OH− + O2 | (18) |
Eqn (17) indicates the process of hydroperoxide reduction, and eqn (18) shows hydroperoxide disproportionation during the 2-e− transfer mechanism. The orientation of the catalyst is crucial for enhancing the efficiency of ORR, given that it is a kinetically sluggish process under normal conditions and can undergo either a 2- or 4-e− transfer process.
Although Al–air batteries rely on ORR at the cathode, the kinetics of this reaction have to be a 4-e− transfer process to work effectively, particularly in alkaline electrolyte. The 2-e− transfer process in ORR will make the battery less efficient given that it will undergo the formation of peroxide ions (according to eqn (14) and (15)). Considering this, when testing ORR, the number of electrons involved in the mechanism should be close to 4. Thus, improving the efficiency and kinetics of ORR is crucial for maximizing the overall performance and energy density of Al–air batteries.118 Noble metal catalysts including platinum-based materials and their alloys are generally considered active catalysts to promote ORR. However, the high cost of these noble metals limits their use in Al–air batteries and large-scale application.119 Thus, alternatives to noble metals have been explored recently, and their further discussion will be presented in Section 6.
In acidic medium:
X + H2O → H+ + XOH + e− | (19) |
XOH + OH− → H2O + XO + e− | (20) |
2XO → O2 + 2XO | (21) |
XO + H2O → H+ + XOOH + e− | (22) |
XOOH + H2O → H+ + O2 + X + e− | (23) |
In alkali medium:
X + OH− → XOH + e− | (24) |
XOH + OH− → H2O + XO + e− | (25) |
2XO → 2XO + O2 | (26) |
XO + OH− → XOOH + e− | (27) |
XOOH + OH− → O2 + H2O + X + e− | (28) |
To improve the efficiency of OER, a catalyst is employed to decrease the overpotential, which is crucial in the determination of the overall efficiency and OER performance of Al–air batteries. This is because it directly impacts the discharge characteristics, energy density, and battery stability. Efficient OER kinetics provide increased oxygen availability at the air electrode, which helps to enhance the power output of the battery at higher discharge currents. The maintenance of an alkaline environment within the battery is critical to facilitate appropriate electrochemical processes and prevent passivation of the Al anode. Efficient OER can contribute to this objective, which also enhances the probability of the activation of reversibility of the Al–air battery. Thus, the selection of OER catalysts that exhibit high activity and stability is important to optimize the overall performance and feasibility of Al–air batteries.
(29) |
B = 0.62nFACO2DO22/3v−1/6 | (30) |
The ORR properties can further be investigated with the help of a rotating-ring disc electrode (RRDE). The following two eqn (31) and (32) are used to obtain the e− transfer number during the process and H2O2 yield curves.124,125
(31) |
(32) |
Tafel analysis can also be employed to investigate the ORR polarisation, which examines the relationship between Jk and overpotential (η). This relationship can be mathematically expressed as the following eqn (33).127,128
η = a + blog(Jk) | (33) |
(34) |
(35) |
Thus, the overpotential η can be calculated by subtracting the reference electrode potential from the observed half-wave potential (Eobs − Eref).
Thus, the calculated electrochemical potential can be converted into the scale of reversible hydrogen electrode using eqn (36).130
ERHE = Eref(obs) + E0ref + 0.059 × pH | (36) |
(37) |
(38) |
Fig. 4 Schematic demonstration of the setup to determine the hydrogen evolution rate.115 |
The battery efficiency of the Al–air cell is tested in a complete cell composed of an Al anode, a catalyst supported with a current collector, and electrolyte. The main physical quantities to test the efficiency of a complete cell are specific capacity, i.e., capacity per unit mass consumed (Q), Al anode utilization amount (Ua) in percent, and energy density (W), calculated according to eqn (39)–(41):134,135
(39) |
(40) |
(41) |
Further, to analyse the performance of the battery, i.e., parameters such as specific capacity and energy density are crucial. These physical parameters will assist in understanding whether the fabricated battery is efficient. The main attributes such as discharge current, operating voltage, discharge time, and consumed mass of the anode are used to understand the battery performance. The specific capacity is calculated in units of mA h g−1. The discharge current, operating voltage, and discharge time are measured during the controlled battery discharge measurement. Further, to measure the consumed mass, the byproduct from the discharged anode needs to be etched with proper care, which is essential for the precise measurement of specific capacity and energy density. There are various techniques reported in the literature, i.e., etching with strong bases such as NaOH and KOH, chromium oxide, and silver nitrate.111,136,137 Linjee and Ren et al. used 2 wt% Cr2O3 and 5 wt% H3PO4 with DI water at 80 °C for a few minutes to remove the corrosive products.138,139 Some reports also followed the ASTM-G-03 standard, where the consumed anode is rinsed to separate the corrosive byproducts.140,141 However, the used etchant can also etch some of the non-consumed aluminum during the removal of byproducts. Also, the formed byproducts are usually Al(OH)3 or aluminates, which may stick to the surface of Al and increase the mass of the anode. These aspects will tend to provide false interpretations for the measured specific capacity, and thus the measured energy density may not reflect the correct energy density. Thus, it becomes necessary to innovate a particular method for the complete removal of byproducts from the discharged anode to accurately determine the anode utilization, specific capacity, energy density, and other related parameters.
Reboul et al. proposed a dissolution–redeposition method, aiming to address the issue of passive oxide film formation by utilizing aluminum alloying. This method involves the simultaneous dissolution and oxidation of individual elements in the Al matrix, producing cations in the electrolyte, which are subsequently deposited back on the Al surface through electrochemical reactions, which help break the compact oxide layer and activate the Al surface, as presented in Fig. 5(a). It has been suggested that elements with low-temperature eutectic should be selected to fully realize and comprehend multi-element alloying. The separated oxide coating produced by the eutectic development on the Al surface acts as an active site for the breakdown of the alloy. When complexes with cations are formed, the production of eutectic increases the adsorption of anions, which results in pitting corrosion. The amount of amalgam and other eutectic formed on the surface of the Al matrix is of the utmost importance for activation (see Fig. 5(b)). The surface structure of Al alloys during alloying exhibits nonuniformity due to unpredictable processes such as eutectic development, shrinkage, segregation, and imperfections. This non-uniformity may lead to uneven corrosion reactions on the Al surface.77,148 As a result, the surface of Al may experience an uneven corrosion reaction. In addition to other phenomena that may negatively impact the electrochemical performance of the battery, the local corrosion will worsen. Thus, to prevent this, numerous researchers are currently reintegrating the structure of aluminum alloy using an additional element distribution state, and some recent studies are tabulated in Table 3.
Fig. 5 (a) Schematic diagram explaining the dissolution–redeposition mechanism in Al-alloys proposed by Reboul et al. (b) Schematic diagram showing the eutectic mechanism.77,148 |
S. N. | Alloy | H2 evolution rate (mL min−1 cm−2) | Ecorr (V) | jcorr (A cm−2) | Performance (mA h g−1) | At current density (mA cm−2) | Anodic efficiency (%) | Ref. |
---|---|---|---|---|---|---|---|---|
1 | Al–Ga | 0.061 | −2.023 | 2.45 | 2584.1 | 5 | 61.5 | 149 |
2 | Al–In | 0.006 | −1.980 | 0.263 | 3343.2 | 5 | 73.1 | |
3 | Al–Sn | 0.001 | −1.857 | 0.37 | 3267.6 | 5 | 86.3 | |
4 | Al–1Zn–0.1In–0.1Sn–0.5Mg–0.1Mn | 0.128 | −1.776 | 0.0032 | 1481 | 20 | 49.75 | 146 |
5 | Al–1Zn–0.1In–0.1Sn–0.5Mg–0.2Mn | 0.227 | −1.707 | 0.0010 | 1347 | 20 | 45.23 | |
6 | Al–1Zn–0.1In–0.1Sn–0.5Mg–0.3Mn | 0.313 | −1.653 | 0.015 | 1212 | 20 | 40.70 | |
7 | Al 6061 | — | −1.386 | 0.126 | 624.77 | 2.6 | — | 142 |
8 | Al 8011 | — | −1.386 | 0.141 | 628.41 | 2.6 | — | |
9 | Al 1200 | — | −1.420 | 0.073 | 1096.84 | 2.6 | — | |
10 | Al–0.1Sn–0.08Ca | 0.142 | −1.832 | 0.0036 | 2495.75 | 40 | 83.75 | 150 |
11 | Al–Mn–Sb | — | −1.736 | 0.00137 | 2797 | 120 | 93.8 | 151 |
12 | Al–Mg–Sn–In | — | −1.57 | 0.0026 | — | — | 42.7 | 152 |
13 | Al 6061 | 0.3928 | −1.380 | 0.168 | — | — | — | 153 |
14 | Al 8011 | 0.2771 | −1.450 | 0.144 | — | — | — |
Pino et al. investigated commercially available Al-alloys, Al 2024, Al 7475, and Al 1085, as anode for Al–air batteries in both clad and unclad states. The abbreviation used for clad and unclad Al 7475 is Al7C and unclad Al7U, respectively. Similarly, the terms Al2C and Al2U are used in Fig. 6(a) and (b) for the clad Al 2024 and unclad Al 2024 samples, respectively. Fig. 6(a) and (b) illustrate the galvanostatic discharge curves and electrochemical performance in realizing the effect of using alloys in the clad and unclad states as an Al anode, respectively.144 The clad alloys exhibited a superior current discharge at lower current rates. Al 7474 is a commercial alloy, mainly doped with Zn and Mg, which showed improved ability to dissipate current, even at higher discharge currents. The underlying mechanism for this phenomenon is the galvanic coupling between Al and metallic alloying, which influences its surface reactivity with the electrolyte. The alloying of gallium shows acceleration in the active dissolution of the Al anode with Mg and Sn, as described by Wu et al.154 Furthermore, adding indium causes discharge products (such as In and In(OH)3) to emerge, preventing the self-corrosion reaction. Thus, Al–Mg–Sn–Ga–In alloy-based anodes are promising at higher discharge rates for Al–air batteries in brine electrolytes. The polarization curve is shown in Fig. 6(c) for the Al–Mg–Sn–Ga–In alloy in 2 M NaCl electrolyte. Alloys 1, 2, 3, and 4 mentioned in Fig. 6(c) are the combination of Al–0.5Mg–0.1Sn, Al–0.5Mg–0.1Sn–0.05In, Al–0.5Mg–0.1Sn–0.05Ga, Al–0.5Mg–0.1Sn–0.05Ga–0.05In, respectively.154 Ren et al. investigated three different Al–Sn, Al–Mg, and Al–Mg–Sn alloys and compared them with pure Al. The results of the self-corrosion test, i.e., potentiodynamic polarization and galvanostatic discharge curves, suggest that alloying resulted in a better battery performance than pure Al. The self-corrosion was maximum for pure Al, followed by Al–Sn, Al–Mg–Sn, and Al–Mg alloys, showing lower self-corrosion with minimal self-corrosion for the Al–Mg alloy. The capacities were 2563 mA h g−1 for pure Al 4N6, 2569.5 mA h g−1 for Al–Sn, 2723.7 mA h g−1 for Al–Mg, and 2661.1 mA h g−1 for the Al–Mg–Sn alloy anodes.155 Further, doping with manganese (Mn) increased the specific capacity to 1500 mA h g−1 by reducing the self-corrosion, resulting in an improved working potential and energy density for ∼50% anode consumption. The corresponding polarization curve is shown in Fig. 6(d). The alloying process involves bonding two distinct metals, modifying their structural integrity and enhancing their electrochemical performance.146,155 This is achieved by carefully selecting the doped metal composition in a proportional ratio based on the desired objective of either preventing self-corrosion or achieving simultaneous current discharging performance. Thus, a suitable alloying composition is essential to achieve the optimal performance of Al–air batteries. Thus, alloying of aluminum anodes offers promising advancements for Al–air batteries, and the ongoing research efforts are aimed at optimizing the alloy compositions and structures for improved electrochemical performances.
Fig. 6 (a) Galvanostatic discharge at 1.6 mA cm−2 and (b) galvanostatic discharge at 3.2 mA cm−2 of the Al 2024 and Al 7475 alloys in the clad and unclad states, respectively.144 (c) Polarization curves of alloys in 2 M NaCl electrolytic solution of alloy 1–4 at 0.167 mV s−1 for 30 min.154 (d) Potentiodynamic polarization curves of the Mn-doped alloy (Al–1Zn–0.1In–0.1Sn–0.5Mg–xMn) anodes in 4 M NaOH solution at 1 mV s−1 for 60 min.146 |
Fig. 7 Pourbaix diagram for aluminum, which is used to understand its possible corrosion, passivation, and immune regions in water medium.73 |
The various types of electrolytes are explored in the aqueous medium of different pH for Al–air batteries. The most common electrolytes are alkaline-based aqueous medium to promote ORR, as discussed in Sub-section 3.2.158 Efforts are devoted to changing the pH with additives, which will mitigate the limitations associated with alkaline-electrolytes. These alkaline aqueous electrolytes in Al–air batteries are widespread due to their superior ionic conductivity. The stability of a metal is mostly constrained in acidic environments, which is why either alkaline or neutral electrolyte is preferred in the metal–air batteries. Both alkaline and neutral media have been suggested given that they have similar reaction pathways for oxygen redox activities (as discussed in Sections 3.2 & 3.3). However, it has been observed that the kinetics of these processes are relatively slower in neutral electrolyte, which poses a considerable constraint on the performance of Al–air batteries. The most well-known electrolytes for Al–air batteries are KOH and NaOH in alkaline electrolyte.159,160 KOH is also preferred over NaOH due to its faster kinetics, better conductivity, and higher diffusion coefficient. However, NaOH is mainly used because KOH solution hinders recycling via the Hall–Héroult process.161
KOH and NaOH electrolytes exhibit a reduced voltage and current output with time compared to NaCl electrolyte. The initial OCP for the alkaline medium is relatively higher; however, it degrades very quickly. As the number of OH− ions in the electrolyte increases, the anode will generate more metal oxide. Consequently, electrolyte with a higher OH− concentration will experience rapid depletion compared to that with a lower concentration of OH− ions.162,163 Thus, saline water is considered relatively safer due to its neutrality. However, this is also prone to higher polarization, which causes severe corrosion. The presence of chloride will eventually help in reducing the polarization potential by the absorption of Cl− ions on the anode side.164 However, this will not sustain for a longer duration, and that is why other salts can be employed as an additive, such as sodium hydrogen carbonate and sodium sulphate. These additives will precipitate the gel of aluminum hydrate, which is the main culprit in reducing ionic conduction inside the electrolyte. In the case of crewless underwater vehicles, the choice of electrolyte is seawater itself, given that it is economically viable and requires low maintenance. However, in addition to the aluminum anode, other sub-components of the battery, such as the current collector and housing materials, may be susceptible to corrosion in seawater, which contains Cl− ions, forming acidic byproducts.165 Some of the recent studies related to the electrolytes and additives in aqueous and hydrogel media are tabulated in Table 4.
S. N. | Electrolyte | Additive element | H2 evolution rate (mL min−1 cm−2) | Ionic conductivity (mS cm−1) | Specific capacity (mA h g−1) | At current density (mA cm−2) | Ref. |
---|---|---|---|---|---|---|---|
1 | 4 M KOH | 2 M sucrose | 0.178 | 34.98 | 2330 | 10 | 166 |
2 | 4 M NaOH | 20% glycerol | 0.042 | 86.00 | 2564 | 10 | 167 |
3 | 4 M NaOH | 10 mM ZnSO4 + 1 g per L sodium alginate | 0.174 | 13.82 | 267.41 mA cm−2 (capacity density) | 30 | 162 |
4 | 4 M NaOH | ZnO/glucose | 0.097 | — | 2271 | 20 | 52 |
5 | 4 M KOH | 10% v/v 0.5 M Ba-acetate | 0.042 | — | 2817 | 10 | 168 |
6 | 4 M NaOH | 1.6 g per L zinc oxide + 1.0 mM 8-aminoquinoline | 0.211 | — | 2703 | 20 | 169 |
7 | 4 M KOH | 13 M (CO(NH2)2) | 0.019 | 390.00 | 2330 | 35 | 170 |
8 | 6 M KOH | ZnCl2 | 0.039 | — | 2322 | 20 | 171 |
9 | 4 M NaOH | 4 mM-hexadecyl-3-methylimidazolium hexafluorophosphate (HMIH) | 0.437 | 2128 | 20 | 172 | |
10 | 4 M KOH | 10 mM 4-amino-6-hydroxy-2-mercapto pyrimidine and 4 mM zinc oxide | 0.134 | — | 785 | 20 | 173 |
11 | 4 M KOH | 0.05 M Na2SnO3 and 4 mM ellagic acid | 0.366 | — | 2439 | 50 | 174 |
12 | 4 M NaOH | 1 mM dodecyl dimethyl betaine and 4 mM sodium dodecylbenzene sulfonate | 0.110 | — | 2548 | 40 | 175 |
13 | KF and KOH (hydrogel) | PAA | 0.990 | 371.00 | 2199 | 10 | 176 |
14 | Agar hydrogel | 0.5 M Zn2+ | 0.990 | 215.4 | 2592 | 10 | 177 |
15 | KOH hydrogel | (NH4)2S2O8 in PAA | 0.019 | 397.00 | 2377 | 10 | 178 |
The common problem faced by electrolyte in aqueous medium is that they tend to dissolve CO2, resulting in the formation of carbonate, which hinders the efficiency of the battery.101 These limitations must be mitigated to achieve the maximum anode efficiency. The Al anode naturally tends to form a protective oxide layer when exposed to oxygen and moisture in aqueous medium, which suppresses the overall performance of the battery. Thus, to overcome this, other media such as ionic and gel electrolytes are also explored for use in Al–air batteries.
Gelman and group used 1-ethyl-3-methylimidazolium oligo-fluoro-hydrogenate (EMIm (HF)2.3F) and tested its use in a primary Al–air battery. This material was chosen due to its proven potential in silicon–air battery applications. The electrochemical potential range is the disparity between the limits of the cathodic and anodic peaks, representing the potential values at which oxidation and reduction appear. Finally, the number of electrons (n) was taken 2.3 due to the demonstrated hygroscopicity at n < 2.3. In addition to its stability in moisture and water, this ionic liquid possesses additional beneficial characteristics, such as electrical conductivity of approximately 100 mS cm−1 and low viscosity. Unlike other organic solvent electrolytes, EMIm (HF)2.3F electrolyte can activate aluminum by disrupting its passive oxide layer through a specific species. Ferrocene/ferrocenium (Fc/Fc+) was employed as the reference electrode, which is compatible with the ionic liquid electrochemistry. The experimental findings (−1.1 V for aluminum anode and 1 V vs. Fc/Fc+ for cathode) demonstrated a cell potential of 2.1 V for the Al–air battery. Linear polarisation tests were performed to evaluate the corrosion current density in EMIm (HF)2.3F. The current density of ∼25 μA cm−2 is insignificant compared to the corrosion current density recorded in aqueous alkaline electrolyte. The results of the discharge studies conducted at current densities in the range of 0.1–1.5 mA cm−2 indicated that the aluminum foil anode exhibited a max charge capacity of 160 mA h, which is lower than the calculated capacity of 227 mA h. The morphology of the anode surface showed that the diameter of the pores formed due to aluminum dissolution increased with an increase in the discharge current density. Specifically, the diameter ranged from 20 to 50 nm at a current density of 0.1 mA cm−2 compared to a diameter of 200 to 400 nm at a current density of 1.5 mA cm−2. The ionic liquid electrolyte-based Al–air battery demonstrated 70% of the predicted discharge capacity and a remarkably low corrosion current density.183
Fig. 8 (a) Optical photograph of PPM-0.3 with a weight resistance of up to 100 g. (b) Mechanical illustration of the process for the synthesis of PPM gel. (c) Electrochemical analysis with the power density and discharge curve to test the change in bent state vs. normal state of gel PPM-0.3.185 |
Ryohei Mori demonstrated a solid-state rechargeable-type Al–air battery. He mixed AlCl3, urea, CMC, and glycerin in a 3:2:1:1 molar ratio as the electrolyte and soaked it in commercial gauze during the process of charging/discharging the solid-state Al–air battery. The applied current rate was 0.1 mA cm−2, with a cutoff potential in the range of 0.2–1.5 V. The initial capacity of the cell was 35.8 mA h g−1, which retained ∼35.0 mA h g−1 after 50 charge–discharge cycles, exhibiting 97.8% capacity retention. Here, the air cathode used TiN, a suitable catalyst for promoting ORR. It is worth noting that neither Al2O3 nor Al(OH)3 was formed as a byproduct. The other byproducts formed did not cause any hindrance in the reaction kinetics.186 Xu and group directly demonstrated a fiber-embedded Al–air battery in a wristwatch. This demonstration showed flexibility and proposes a way to maintain it during application. The solid-state polymer electrolyte was comprised of PVA and PEO mixed in KOH aqueous solution together with ZnO and Na2SnO3 additives. Here, a spring-shaped anode was considered with the electrolyte, which cross-linked the anode spring via the freeze-thawed method. The air cathode was conjugated with Ag nanoparticles coated with CNT and covered on a Teflon plate. The flexible solid-state battery exhibited a practical energy density of about 1.17 kW h kg−1 and a specific capacity of 12 A h g−1. However, the rechargeability was not demonstrated for this cell.187
ZnO has been researched as an additive in alkaline electrolyte.169 Thus, it is worth checking the performance of ZnO with other inhibitors to enhance the potential of Al–air cells. Wang et al. developed a non-ionic surfactant branched alkyl glycoside (BAG) and ZnO-based hybrid inhibitor, and the respective inhibition mechanism is illustrated in Fig. 9(a). ZnO has a mild inhibitory effect on aluminum corrosion because of its corrosion-resistant characteristics. Further, in the case of the BAG/ZnO hybrid inhibitor, the BAG molecules attach to the Al surface and organize themselves into structured molecular arrays, as explained schematically in Fig. 9(a). The oxygen functional groups primarily occupy the active sites for hydrogen evolution, while the hydrocarbon chains protect the Al base from the surrounding solution. The Zn2+ ions form a molecular network by interacting with the –OH groups on the glucoside. Simultaneously, a few Zn2+ ions move across the network, filling the positions between molecules. The glucoside–Zn coordination complex functions as a structural foundation for the deposition of Zn, thereby accounting for the consistent distribution of Zn nanoparticles. In addition, the presence of glucoside–Al bond anchors inside the network enhances the stability of the protective layer. This is also visible in the electrochemical performance in Fig. 9(b)–(e). According to Fig. 9(b), it can be observed that the initial passivation potentials of the hybrids exhibit a negative shift compared to the passivation potential of ZnO alone of −1.196 V. Moreover, the density shoulders observed in the hybrids exhibit a notable decrease compared to that observed in ZnO only. This indicates that BAG can expedite the deposition of Zn and enhance the density of the protective layer. The discharge curve of a complete Al–air battery for 12 h at a current density of 20 mA cm−2 is shown in Fig. 9(c) to test the impact of the electrolyte on the discharge performance. The voltage at which ZnO and the hybrid electrolytes operated seemed to decrease as the depth of discharge increased. The observed phenomenon can be attributed to the buildup of byproducts on the anode. The battery containing ZnO demonstrated fluctuations in battery voltage, which was attributed to the ongoing process of Zn layer deposition and stripping. The addition of BAG with ZnO in the electrolyte solution resulted in a significant reduction in these fluctuations. Upon addition of the hybrid of 0.2 M ZnO and 20 g per L BAG, the specific capacity reached 2396 mA h g−1, which was ∼1253 mA h g−1 without any additive at the same current (Fig. 9(d)). Furthermore, a series of discharge experiments was conducted at various current densities in the range of 5–25 mA cm−2 to assess the viability, as presented in Fig. 9(e). This finding demonstrates that the incorporation of BAG can significantly augment the stability of the protective layer.189
Fig. 9 (a) Schematic illustration of inhibition mechanism ZnO/BAG. (b) Polarization curves of Al in 4 M NaOH electrolytic solution with and without inhibitor. (c) Discharge curves at 20 mA cm−2 for 12 h. (d) Discharge curves at 20 mA cm−2 for 2 h using hybrid electrolytes. (e) Discharge curves at 10–25 mA cm−2 with the hybrid of 0.2 M ZnO and 20 g per L BAG.189 |
The active layer of the catalyst is composed of the active material, acetylene black, and binder dissolved in N-methyl-2-pyrrolidone (NMP). The catalytic ink is usually applied on the current collector on the air cathode side. It serves as the site for ORR to trigger the reaction. The electrocatalyst present in the air electrode is crucial in defining the performance of the electrode and maximizing the energy density. The effectiveness of the Al–air battery is determined by the efficiency and rate of electrochemical ORR at the cathode. These properties can be enhanced by customizing the cathode catalysts via nanoengineering. The limited practical application of the Al–air battery is primarily due to the sluggish ORR at the cathode. In this case, despite their high cost and limited availability, platinum and its alloys are widely recognized as the most effective electrocatalysts for ORR in alkaline aqueous solutions. Nevertheless, the successful execution of commercial applications necessitates an economically feasible and environmentally sustainable catalyst. Also, the particle shape and exposed surface are critical in determining the catalyst performance.57 A positive correlation exists between the response rate and the extent of exposure to the catalyst surface. For the feasibility of an Al–air battery, the air cathode must incorporate an appropriate electrocatalyst to modify its ORR activity. The different types of catalysts used for Al–air batteries are discussed in the following sub-sections.
Despite the numerous hurdles associated with Pt catalysts, such as the need to regulate their facet distribution and manage their particle size, the primary issue stems from the high cost and limited availability of Pt as a finite natural resource. Hence, it is crucial to develop Pt-based catalysts that exhibit high efficiency while minimizing the Pt loading. In this case, one viable approach involves the loading of Pt on catalytic substrates with substantial surface areas. Wang et al. described that the catalytic efficiency of Pt alloys can surpass that of pure Pt. That occurs due to the phenomenon involving a reduction in the size of the Pt lattices and modification of its d-orbital states by the incorporation of transition metal atoms.194 This enables the attainment of higher catalytic activities compared to pure Pt. The catalytic activity of Pt metal catalysts is also influenced by various factors such as their particle size, structure, chemical composition, and electronic structure when combined or doped with other metals. Pt was also integrated with different transition metals to examine their impact on Pt alloys. For example, a 9 nm octahedral Pt–Ni catalyst exhibited favorable catalytic performances.195 Also, octahedral Pt–Ni nanoparticles displayed enhanced ORR activities compared to cubic-structured Pt–Ni nanoparticles.196 This implies that the catalytic activity is significantly influenced by the size and crystalline structure of Pt. However, despite the excellent performance, it is important to note that the catalytic activities may degrade over extended periods due to the limited durability of mixed transition metals. Thus, to mitigate this, some researchers have suggested the use of core–shell-structured catalysts, limiting the amount of Pt employed on the surface and protecting the transition metals on the catalytic surfaces.197–201 Luo et al. synthesized a catalyst with Au nanoparticles with Pt loaded on MWCNT using a one-pot synthesis method. Among the different ratios of Au and Pt, the optimized slurry was a 10.2 wt% slurry of Au:Pt in the ratio of 0.67:1, exhibiting excellent ORR activity and durability with 20 wt% Pt/C. Further, with an increment in the amount of Au:Pt (1.68:1), the specific capacity and power density increased to 921 mA h g−1 and 1486.8 mW cm−2, respectively.103
A nanoporous gold nanoparticle catalyst was prepared through the dealloying of gold–silver leaves by M. Wang and coworkers. They claimed that this catalyst is 55 times cheaper than Pt/C. This promising catalyst could minimize the overpotential to 56 mV dec−1, which was 78 mV dec−1 in the case of Pt. Its stability was also comparable to that of Pt/C. However, the difference can be seen in the sample preparation using chemical and electrical dealloying together with and without surfactants. The difference in the orientation of the facets was suggested to be responsible for the change in ORR behavior. Theoretically, (100) facets are likely to be more electrochemically favorable for ORR.104
Among the metals, Ag also seems to be a good option for utilization as a catalyst due to its impressive conductivity and low cost compared to Pt and gold. However, Ag powder suffers from weaker oxygen adsorption, creating hindering its catalytic behavior. Hong et al. developed a silver catalyst on carbon fiber paper without using a binder, which was deposited via in situ electrodeposition. The calculated Tafel slope was around 98 mV dec−1. At a current density 30 mA cm−2, the silver catalyst demonstrated a very high specific capacity of more than 2780 mA h g−1 and an energy density of 4342.3 W h kg−1. The demonstrated capacity is quite close to the theoretical capacity of the Al-anode.202 Wang et al. prepared Ag–Cu alloy nanoparticles using hot-arc plasma technology.203 The synthesis procedure is illustrated in Fig. 10, where the N-doped porous nanocarbon was mixed via wet grinding to enhance its conductivity. Ag and Cu both are known for their catalytic properties. Thus, alloying of both particles is expected have a synergistic effect. Further, the addition of N-doped nanocarbon tends to provide more active sites for ORR. The rapid heating and cooling process caused it to form a eutectic mixture of Ag–Cu, which changed its inert electronic structure. The prepared structure was a 3-D porous structure with a surface area of ∼400 m2 g−1 and an average pore size of 2.77 nm.
Fig. 10 Schematic illustration of the synthesis of Ag–Cu nanoparticles.203 |
Different compositions of Ag–Cu were evaluated electrochemically, as shown in Fig. 11(a)–(e). Among the prepared catalysts, the Ag–Cu25/NPC catalyst exhibited the maximum ORR peak voltage of 0.80 V, which was ∼50 mV lower than the Pt/C peak potential of 0.84 V, as can be seen in Fig. 11(a). The peak potential of the ORR for Cu/NPC was 0.78 V, which is greater than that observed for Ag/NPC of, but the peak potential of AgCu25/NPC was 0.77 V, falling between them. According to the LSV curve in Fig. 11(b), AgCu25/NPC showed a half-wave potential, the second highest after Pt/C. Also, the number of electrons was 3.9, which is comparable with that of Pt/C (3.89), and H2O2 was suppressed by up to 7.93% (Fig. 11(c)). Similarly, it can be inferred from the Tafel slope and plot of current density as a function of scan rate, as shown in Fig. 11(d) and (e), respectively, the AgCu25/NPC composition is the most favorable. Subsequently, utilizing the AgCu25/NPC catalyst, the fabricated Al–air battery demonstrated remarkable electrochemical capabilities. It achieved a power density of around 191 mW cm−2, maintained a good current output, and sustained a stable high voltage for 120 h. These results highlight the significant potential of this battery to serve as a viable alternative to conventional Pt/C catalyst-based batteries.203
Fig. 11 Electrochemical performance of different compositions of catalysts in 0.1 M KOH O2/N2-saturated electrolyte using RDE. (a) Cyclic-voltammetry curves, (b) linear sweep voltammetry curves, (c) electron transfer number, n, and hydrogen peroxide yield, (d) Tafel slopes, and (e) current density as a function of scan rate at 0.4 V vs. RHE.203 |
Fig. 12 (a) SEM micrograph of carbon aerogel showing its porous network of microspheres. (b) Nitrogen-adsorption isotherm to evaluate surface area. Comparison of the electrochemical activity with carbon aerogel and without carbon aerogel using (c) linear sweep voltammetry curve and (d) discharge performance at 1.275 mA cm−2.210 |
Liu et al. added graphene oxide in an Mn-based catalyst to improve the catalyst response and compared the Mn-catalyst with the composite of graphene oxide-added manganese catalyst (Mn-based @GO) and commercial 20% Pt/C. The discharge voltage of the Al–air battery utilizing the Mn-based catalyst as the catalyst initially dropped rapidly and reached a stable level after 1.5 h, reaching approximately 0.85 V. The Al–air battery, when using the Mn-based@GO catalyst as the air-cathode rapidly reached a stable discharge voltage of approximately 1.26 V. This value closely matched the voltage of the commercial 20% Pt/C cathode, which was 1.28 V. When comparing the Mn-based catalyst to the Mn-based@GO catalyst, the latter enhanced the discharge voltage of the Al–air battery by 0.41 V at a current density of 30 mA cm−2. Additionally, the stability of the Mn-based@GO catalyst was superior. The distinctive form of the Mn-based@GO, which was synthesized using a hydrothermal method using 20% GO, can be attributed to the combined influence of α-MnO2, MnO(OH), and GO. The incorporation of GO resulted in the generation of MnO(OH) nanorods, leading to the synthesis of a new nanocomposite consisting of MnO2/MnO(OH)@GO. The addition of GO in Mn successfully reduced the consumption of aluminum, and the mass-energy density increased from 1485 to 2119 W h kgAl−1. Furthermore, the incorporation of GO significantly enhanced the surface defects in the nanocomposite material, hence facilitating the enhancement of its electrochemical characteristics. In addition, the electrochemical test demonstrated that the incorporation of GO substantially improved the performance of the manganese-based catalyst.214 It has been perceived that adding a graphene oxide-like carbon material may also be useful for other metal and metal oxide-based catalysts. Similarly, Qin et al. added 20% graphene oxide to Mn-doped SrCoO3 (G-SrCo0.5Mn0.5O3), exhibiting better electrochemical activity and discharge performance. The discharge power density for SrCoO3 was recorded at 13.26 mW h cm−2, which decreased after adding manganese (SrCo0.5Mn0.5O3) to 12.75 mW h cm−2 and increased after loading graphene to 13.85 mW h cm−2, at a current rate of 10 mA cm−2.215
Directing the catalytic activity of any material depends on it electrochemical selectivity. Some recent works and their results are summarized in Table 5, highlighting electrochemical parameters, including Eonset, E1/2, Tafel slope, OCP, and performance.
S. N. | Catalysts | Eonset vs. RHE (V) | E1/2 vs. RHE (V) | Tafel slope (mV dec−1) | OCP (V) | Specific capacity (mA h g−1) | Power density (mW cm−2) | At current density (mA cm−2) | Ref. |
---|---|---|---|---|---|---|---|---|---|
1 | LaCoO3 perovskite | 1.124 | 0.929 | 83.7 | 1.35 | 1770 | 10 | 0.33 | 206 |
2 | (Co,Mn)3O4-doped carbon nanotube composite | — | 0.831 | 87.17 | 1.48 | — | 147 | 50 | 216 |
3 | Fe–Cu dual-site nanoparticles | 1.01 | 0.867 | 69 | 1.56 | — | — | 20 | 217 |
4 | NiFe LDH A-FeSACoSA-FeCoAlloy-CNT/NC | 0.93 | 0.86 | 125.5 | 1.49 | 120 mA h g−1 (at 1 mA cm−2) | 145 | 157 | 218 |
5 | Fe/Ce-NCNT | 0.97 | 0.88 | 98 | 1.81 | — | 164 | 100 | 219 |
6 | Mn-based@GO | 0.91 | 0.77 | 112.62 | 1.5 | 1682 (at 30 mA cm−2) | 57 | 50 | 214 |
7 | Fe–Nx@NC/rGO | 1.03 | 0.925 | 58.99 | 2.01 | 2584 (at 100 mA cm−2) | 98 | 150 | 212 |
8 | Ag–Cu25/NPC | — | 0.82 | 79 | 1.89 | 2412 | 193 | 120 | 203 |
9 | Co@N/GNP | 0.98 | 0.87 | 78 | 1.61 | — | 143 | 191.83 | 220 |
10 | Ag@MnO2/MWNT | — | 0.87 | 106 | 1.68 | 1240 | 140 | 20 | 124 |
11 | Fe–NG–MXene | — | 0.91 | 77 | — | — | 82 | 50 | 221 |
12 | α-MnO2/Co3O4 | 0.833 | 0.76 | 89 | — | 185 | 50 | 222 | |
13 | MnS/NS–C | 1.07 | 0.91 | 58 | 1.56 | — | 135 | 192.3 | 223 |
14 | CoNi@NCNTs/CC | 0.89 | 0.82 | 64 | 1.68 | 1029 | 151 | 221 | 224 |
15 | FePc@HNSC | 0.99 | 0.88 | 77 | 1.92 | — | 205 | 150 | 211 |
16 | 3DOM LSMO | 0.89 | 85.3 | 1.44 | 1084 | 5 | 207 | ||
17 | NiSAFeSA-Ni@FeNPs/CNTs-NGNS | 0.92 | 0.87 | 86.7 | 1.61 | — | 184 | 270 | 225 |
18 | NCAG/Fe–Cu | 1.07 | 0.94 | 55 | 2.00 | — | 137 | 10 | 226 |
19 | 3.5ZnS/NSC-NaCl-900 | 1.02 | 0.905 | 98.3 | 1.71 | 936 | 251 | 50 | 227 |
20 | FeCo/N–C–pistachio | 0.93 | 0.83 | — | — | — | 100 | 10 | 228 |
21 | FeCo/N–C–peanut | 0.91 | 0.71 | — | — | — | 60 | 10 | 228 |
22 | Chem-npAu | 0.93 ± 0.01 | 0.83 ± 0.01 | 57 | — | — | 237 | 360 | 104 |
Elec-npAu | 78 | ||||||||
23 | 0.8-CoNCNT | 0.94 | 0.85 | — | 1.794 | — | 159.6 | 217.8 | 229 |
24 | Au1.68Pt/MWNTs | 1.159 | 0.892 | 74 | 1.75 | — | 146.8 | 200 | 103 |
25 | MnOOH@CeO2 | 0.91 | 0.80 | 111.1 | — | — | 302.8 | 400 | 230 |
26 | Co3Fe7–Fe3C/HNC | 0.78 | 0.64 | 85 | — | — | 210 | 286 | 231 |
27 | reduced m-Co3O4/3DG | 0.93 | 0.84 | 71.45 | 1.53 | 422.74 | — | 1 | 159 |
28 | MnO/Mn2O3/ONCNF-3 | 0.903 | 0.805 | 103.8 | ∼1.8 | — | 129.7 | 165 | 232 |
29 | Fe–SA–NC@CC | 0.97 | 0.86 | — | 1.53 | — | 3.94 | 1 | 233 |
30 | FeNi–NP/NC | — | — | 89 | ∼1.6 | — | 24.9 | 1 | 234 |
Type of electrolyte | Advantages | Disadvantages | Suitable design |
---|---|---|---|
Aqueous electrolyte | • High ionic conductivity | • Limited voltage stability | • System with circulatory pump |
• High discharge performance | • Water management/leakage issues | • Separator soaked with electrolyte | |
• High water content reduces the cost | • Disposal of corrosive products | ||
Ionic electrolyte | • Wide electrochemical stability window | • Limited conductivity | • Separator soaked with electrolyte |
• Minimizing side reactions | • High viscosity | • Polymer-based assembly | |
• Low volatility | • Heavy weight | ||
Solid/gel electrolyte | • Enhanced safety due to no leakage | • Limited ionic conductivity | • Flexible assembly |
• Wide temperature range | •Processing complexity | • Thin batteries as 3-D printed/paper-based | |
•High durability and light in weight | •Instability due to shrinkage over time |
The coin-cell-based assembly is the conventional cell used to check initial results on the lab scale and is suitable for all types of electrolytes. The A-MAD research group used the traditional 2032 coin-cell assembly by puncturing its upper case to make holes for the passage of air.142 A schematic of the assembly is shown in Fig. 13(a). Atencio et al. comprehensively studied aqueous-to-gel electrolytes, additives, and alloys using the design of a polymer-based 3-D printed pattern composed of ABS polymer.110,235 Some researchers use acrylic sheets, as shown by the A-MAD research group, in a similar type of assembly made up of acrylic polymers given that they are not affected by alkaline medium and will run for a longer duration.55 There are some structural differences between the aqueous and gel electrolyte, showing that the assembly in series can withstand a higher voltage load. However, these batteries are often overlooked due to the heavy weight of metals and polymers, which limits their practical applications. Thus, to address the challenges associated with weight, researchers have explored the use of 3-D-printed batteries with ultrathin dimensions to achieve a more compact design.236–239 Wang et al. demonstrated exceptional flexibility in their Al–air battery design, allowing for various use cases and physical bending without performance degradation. They developed a cellulose-paper-based Al–air battery. An Al foil anode was used inside the cellulose substrate, while the air-cathode was applied on its surface using catalyst ink to realize the complete Al–air cell. A detailed schematic is presented in Fig. 13(b). With its uncomplicated design and affordability, the Al–air battery exhibited a commendable power density of 19 mW cm−2 in alkaline electrolyte, but its operational time was just 48 min. Furthermore, a test was conducted with saline electrolyte, showing an operational longevity of up to 58 h at 1 mA cm−2, and only 25 mg of aluminum could be recovered. The specific capacity of aluminum is reported to be 2338 mA h g−1. This battery demonstrated exceptional flexibility when subjected to various bending angles and repeated bending cycles exceeding 1000 cycles.237 Another study utilizing the jet printing technique to reduce the thickness involved the preparation of an ultrathin electrolyte using aerosol printing. PVA was utilized as the gelling agent, while 1.8 M NaCl was employed as the salt supply. A flexible Al–air battery was constructed using an ultrathin electrolyte, with carbon cloth as the air cathode and aluminum foil as the anode. The cell pack weighed approximately 115 g and was less than 1.3 mm thick. A schematic of the battery is presented in Fig. 13(c), which could be fastened to the skin or clothing surface based on specific requirements. The cell pack employed in this study utilized a flexible ultrathin-neutral electrolyte, mitigating the chances of electrolyte leakage. The cellular arrangement was affixed to a muscle sticker, and the aluminum anode was not in immediate proximity to the skin, ensuring safety concerns. The discharge performance was tested at different electrolyte thicknesses with a combination of varying current densities from 0.1 to 1 mA cm−2. The best discharge capacity of about 2011 mA h g−1 was observed at 1 mA cm−2 with a thickness of 74.5 μm. When checking the discharge performance at intervals of 30 min, the specific capacity was ∼1506 mA h g−1 at 0.5 mA cm−2 for the electrolyte thickness of 37.8 μm. These studies show the perfect use of these thin and flexible batteries in various portable, wearable, and point-of-care applications. However, the removal of the Al2O3 oxide layer on the surface of the Al anode is challenging when using neutral electrolyte. The concentration of Cl− ions is restricted in a thinner electrolyte. During the electrochemical reaction, the Al anode will dislodge the Al2O3 shell, which will accumulate at the interface between the electrode and the electrolyte. This accumulation will increase the internal resistance of the battery and hamper the movement of ions. Furthermore, the presence of Cl− ions in the denser electrolyte is adequate for their penetration in the surface of the Al anode, enabling their active involvement in the electrochemical reaction.240
Fig. 13 (a) Coin-cell 2032-based assembly with battery components of Al–air battery.142 (b) Process for the fabrication of 3-D printed paper-based Al–air battery.237 (c) Schematic illustration of 4 cell pack ultrathin Al–air battery made up of solid-electrolyte using aerosol jet printer.240 (d) Schematic image of the dual-electrolyte system consisting of liquid anolyte and gel catholyte.242 (e) Schematic illustration of AGE-based flexible wearable Al–air battery.243 |
Pan et al. created a cotton-based Al–air battery using a low-cost industrial-grade Al plate as the anode. The selection of cotton as the substrate was based on its superior electrolyte storage capacity and reduced resistance to ion diffusion. Furthermore, a precise quantity of solid alkaline was pre-applied within the cotton material to regulate the ability of the battery to release energy and improve user safety. Besides, a passive water reservoir was utilized to maintain the required level of wettability. A ‘passive water reservoir’ is a reservoir that maintains the required level of wettability without active pumping. Additionally, pre-storing solid alkaline electrolytes in cotton enables secure operation and precise regulation of the discharge capacity. Consequently, this results in the development of a very practical power source suitable for applications that do not require much power. Furthermore, self-corrosion is effectively suppressed due to the impediment of OH− dispersion within cotton. The cotton-based Al–air battery system demonstrated a significantly elevated peak power density of 73 mW cm−2. In addition, a notable specific capacity of 940 mA h g−1 and substantial specific energy of 930 mW h g−1 were achieved at a current density of 10 mA cm−2. Its voltage output may be effectively enhanced by developing a multi-cell battery pack. The affordability and sustainability of this battery technology make it particularly well-suited for recharging a range of mini-electronic devices in outdoor settings, where access to the electrical grid is limited and energy density is a critical factor.241
Phusittananan et al. demonstrated a dual electrolyte system-based Al–air battery, as illustrated in Fig. 13(d). In the case of dual electrolytes, it is necessary to store one a separate system. The substances used as anolytes in this study consisted of ethylene glycol/ethanol solutions (0, 5%, 10%, 20%, and 30% v/v), which were combined with 3 M potassium hydroxide (KOH). The catholyte utilized in this study is a polymer gel electrolyte known as Carbopol® 940. Given that one electrolyte is aqueous and the other is a gel, a circulatory pump is attached to the aqueous anolyte to minimize Al corrosion, triggered by HER. These findings indicate that utilizing the dual-electrolyte Al–air flow battery can effectively mitigate anodic corrosion and passivation, contributing to an improved battery performance and longevity. However, the sluggish reaction kinetics could not be completely resolved.242
The management and utilization of liquid alkaline electrolytes pose significant challenges in the context of wearable power supplies. Al–air batteries with a semi-open layout can cause battery degradation and severe burns to the human skin due to the leakage of the electrolytes and alkali escape. Thus, the outdoor use of these battery assemblies is contingent on the resolution of this complex matter. To show the battery application in wearable and portable devices, Sun et al. developed a flexible battery. A high-strength agarose gel electrolyte (AGE) was developed to create a wearable battery with excellent energy density, safety, and significantly reduced self-corrosion. This AGE has a combination of outstanding strength and remarkable capacity to withstand alkaline solutions. The high-toughness AGE exhibited exceptional resistance to deformation under high pressure, preventing any electrolyte leakage (Fig. 13(e)). It ensured a stable interface between Al and AGE, facilitating the attachment of the passive layer to the Al anode surface and effectively preventing self-corrosion. The use of AGE reduced the self-corrosion rate of Al by up to 402% compared to solution-based alternatives. Significantly, the soft-package Al–air battery with a surface area of 10 cm2 exhibited a discharge endurance of 20.1 h and a remarkable specific capacity of 2148.5 mA h g−1. A wearable Al–air battery pack with practical utility was additionally equipped to power an LED array and a smartphone for practical applications.243
The aqueous electrolyte is mandatory for a higher operating voltage in Al–air batteries. However, it is restricted given that the anode continues to corrode when the battery is not in use because of the continuous contact of the anode with the electrolyte. A schematic of the conventional aqueous electrolyte with a circulatory pump is shown in Fig. 14(a). Considering this issue, especially with aqueous electrolytes, Hopkins et al. provided a solution.244 The mitigation of open-circuit corrosion was achieved by replacing the electrolyte on the electrode surface with a nonconducting oil during the off-battery phase. Oil displacement with electrolyte facilitated the battery discharge, resulting in an enhanced power and energy density. The ability of the proposed cell surfaces to exhibit underwater-oleophobic wetting characteristics enabled the reversible displacement of oil (see Fig. 14(b)). For this purpose, they measured the advancing and receding underwater contact angles of silicone oil and PFPE oil on the Celgard separator and the Al electrode. When exposed to water on the Al electrode, both silicone and PFPE oil exhibited oleophilic properties. However, the silicone oil caused the Celgard to wet, whereas the PFPE oil formed beads on the hydrophilic PTFE separator. During the on–off cycles, the current rate was 150 mA cm−2 for 25 min, with a 1 h interval during the rest state. Following the injection of silicone oil, the successive expulsion voltages exhibited a negative value, showing that the silicone oil caused fouling in the Celgard separator. The silicone-Celgard combination resulted in a total energy density of 0.66 ± 0.08 W h gAl−1. In contrast, the PFPE–PTFE combination resulted in a total energy density of 3.55 ± 0.08 W h gAl−1, similar to that obtained from charging the battery without any interruptions and without the addition of oil. Thus, the combination of PFPE–PTFE may be helpful in practical applications with the successive mitigation of Al corrosion, achieving high utilization efficiency.244
Fig. 14 (a) Schematic of conventional electrolyte with circulatory pump. (b) Oil displacement method during on/off state connected with circulatory pump.244 |
Most of the reported studies on aluminum rechargeable batteries used non-aqueous electrolytes, which may be eco-toxic and show unstable cyclability. Also, the energy density of these cells is very poor. Furthermore, the use of organic electrolytes poses certain issues related to recycling, sustainability, and large-scale production. Although the water on anodes in metal–air batteries can have adverse effects, it is advantageous and essential for cathodes due to its facilitation of efficient oxygen cathodic reactions. These reactions occur during both the release of oxygen and the charging process. Additionally, water aids in the effective diffusion of ions towards the catalytic sites. A dual electrolyte system made up of alkaline and acidic electrolytes was also used to demonstrate rechargeability.246 Concerning all these facts, Gaele et al. demonstrated the viability of recharging Al–air cells using a dual electrolyte system based on water–gel electrolytes using polymers PVA and xanthan-gum without any separator. PVA–HCl was used as the anolyte, whereas Xa–KCl was used as the catholyte. In the configuration of dual-electrolyte, the water content was lower for the anolyte and higher for the catholyte. The electrochemical characterizations were separately performed in three-electrode systems for the anode and cathode. The results indicated that the anodic potential remained constant for the initial four cycles of charging. Moreover, the variations in anode potentials during charge–discharge were minimal with a difference of 50 mV. The charging potential exhibited an upward trend towards negative values, which indicated a diminished efficiency, while the deposition of aluminum. The discharge potentials stabilized at a constant value and maintained a steady discharge performance. The cathode discharge potentials exhibited a symmetric pattern for the initial six cycles. Besides, there was a notable increase in the variability in charge–discharge potentials of the cathode. The observed trend of the cathode charge shifted the voltage towards the positive direction similar to the behavior of the anode potential. This phenomenon is likely linked to the re-deposition of aluminum.109 However, although rechargeability was shown in these systems made up of dual-electrolytes, to achieve better cyclability and stability, other combinations of catholytes and anolytes need to be explored.
Similarly, a tri-electrolytic system with the integration of polymer ion-exchange membranes, organic electrolytes with alkaline anolyte, and acidic catholyte, reaching an excellent OCV of 2.2 V was reported by Wang et al. By appropriately arranging two ion-selective membranes, the occurrence of acid–base neutralization was effectively prevented, ensuring a consistent battery performance. A schematic representation of the complete system and camera image is shown are Fig. 15(a) and (b), respectively. The anode utilized in this study was standard kitchen aluminum foil. The three chambers of the cell, containing the NaOH/CH3OH anolyte, NaCl/H2O as the bridge electrolyte, and HCl/H2O catholyte, were segregated through the implementation of a robust alkali Cl− exchange membrane and a strong acid Na+ exchange membrane. The air-breathing cathode employed was a GDE with Pt/C catalyst. By utilizing organic anolyte in a targeted manner, the parasitic hydrolysis reaction linked to the oxidation of aluminum was nearly eradicated. The substitution of the alkaline catholyte with acidic catholyte resulted in a 0.83 V increase in the potential for ORR. As shown in Fig. 15(c), the polarization of each component of the cell was investigated. Anodic polarization usually causes the observed difference between OCP and theoretical cell voltage. Here, it was also verified from the polarization of Al that its change in voltage is ∼0.9 V, which implies that nearly half of the voltage drop is because of the anode itself. That can be attributed to the consumption of hydroxide ions in the electrolyte during the formation and limited mass transport. The cathodic polarization predicts the GDE drop, which seems to be caused by sluggish ORR kinetics. It can be expected that the polarisation across both membranes exhibits a predominantly linear pattern. The potential across the Na+ exchange membrane was in the range of 0.1 to 0.6 V, while the potential across the Cl− exchange membrane demonstrated a minor variation from 0 to 0.2 V. Therefore, the potential reduction of 0.7 V and 0.2 V was attributed to the overpotential across both membranes. The conventional Al–air battery with alkaline electrolyte demonstrated a linear polarisation curve characterized by a voltage of 1.5 V and a short-circuit current density (JSC) of 340 mA cm−2. The tri-electrolyte system demonstrated a significantly greater VOC of 2.2 V, while exhibiting a lower JSC of 80 mA cm−2. According to the polarization curve shown in Fig. 15(d), a maximum power density of 60 mW cm−2 was achieved at a current rate of 55 mA cm−2. Also, the hydrogen evolution observed in the conventional aqueous solution was significantly mitigated. The use of an acidic catholyte enhanced the battery voltage to 2.2 V, while resolving the carbonation problems associated with traditional air cathodes. However, after considering the discharge curves in Fig. 15(e), it worked well up to a current rate of 10 mA cm−2, whereas for 15 mA cm−2, the battery performance showed a linear decay.247 Thus, by appropriately arranging the anion and cation membranes, the occurrence of acid–base neutralization was prevented, enabling the achievement of a steady performance, which can be useful for practical applications.
Fig. 15 (a) Schematic setup of the tri-electrolyte system of Al–air battery. (b) Camera image of the assembled Al–air cell. (c) Single-cell electrode polarization of Al, Na+ membrane, Cl− membrane, and GDE. (d) Power density curve of the Al–air cell. (e) Discharge curve of Al–air cell at a current density in the range of 5–15 mA cm−2.247 |
Fig. 16 Fuel energy cycle for Al–air battery applications.248 |
The fuel cycle energy balance consists of four components. These factors include the useful energy stored in the aluminum anodes, the thermal energy generated during the conversion of Al(OH)3 to Al2O3 and Al2O3 to Al; and the unused aluminum that is transformed into the anode plates. The energy density of used aluminum is calculated to be 564 kJ mol−1, which is 72% of its theoretical value of 783 kJ mol−1. Therefore, the useable energy of 0.8 moles of aluminum is 451 kJ.248 Some of the potential practical applications of Al–air batteries are discussed in the following sub-sections.
The prototype of an electric car driven by an Al–air battery was built and successfully demonstrated by the ‘Phinergy’ company in 2013, showcasing the feasibility and potential of this technology for automotive applications.251 Here, each Al plate possesses sufficient energy to transport an EV for an estimated distance of 20 miles. Furthermore, their current system can accommodate 50 plates simultaneously, resulting in a cumulative charge capacity of 1000 miles.252 It is worth noting that this system required water refilling after every 200 miles. In addition, they also developed an EV that uses a combined pack of Al–air and Li-ion batteries. The Al–air battery enhanced the range of the Li-ion batteries by almost six-times. Phinergy also proposed Al–air batteries for short-range aircraft. Thus, Al–air-based energy-storage systems will be beneficial in terms of both weight and expense without compromising the mobility ranges. Recently, Hindalco Industries Limited signed a memorandum of understanding (MoU) with Phinergy to develop and pilot the production of Al batteries.253,254 Here, battery swapping stations, similar to current petrol pumps, are proposed to replace the anode and fill electrolytes. Further, the integration of Al–air batteries into remote sensor networks and surveillance systems may also be realized for longer durations, especially in strategic areas.
Therefore, Al–air batteries appear advantageous due to their lightweight nature and capacity to function under challenging conditions without the risk of flammability, unlike traditional commercial batteries. According to the modern military system, a soldier carries around 70 batteries weighing 7 kg on a mission, as shown schematically in Fig. 17.256,257 The saltwater battery is most suitable for applications with moderate power requirements and where multiple uses are desired, necessitating the emptying and cleaning of the battery between each use. An alkaline electrolyte can be utilized to construct a self-contained, portable battery for satellite communication, offering advantages such as stable performance and extended operational lifespan. The operational specifications necessitated a rapid cold start-up at −40 °C within half-hour, a power output ranging from 6 to 400 W, and an energy density of 435 W h kg−1. The process of battery activation involves the removal of the electrolyte from the reservoirs located at the uppermost part of the cells.120,258
Fig. 17 Equipment carried by a soldier on a mission, with types of batteries used together with their corresponding weight and power ratings.256,257 |
Al–air batteries are also targeted for propulsion in submarines and underwater vehicles, providing electrical power for propulsion motors and onboard systems. The high energy density of Al–air batteries allows underwater vehicles to operate submerged for extended periods without frequent recharging or refueling. The utilization of neutral electrolytes in marine and consumer applications shows excellent potential. Seawater naturally possesses inherent capability to serve as a neutral electrolyte due to its composition of around 3.5 wt% NaCl, conferring a natural advantage to Al–air batteries in underwater applications. Thus, Al–air batteries can be utilized offshore as well using simply Al plates and air cathodes. The electrolyte can be sourced directly from the ocean, resulting in non-toxic by-products and can be immediately released into the sea. Thus, the primary benefit of utilizing neutral Al–air batteries in underwater consumption arises from their exceptional safety features.120
An Al–air battery, which was shaped-like fibers, could be easily manipulated into different forms and flexed at different angles without causing any noticeable structural damage. Ensuring consistent release of fluid during bending and stretching is crucial for practical applications, given that inconsistent release may lead to operational inefficiencies or discomfort, especially considering the dynamic motion of the human body. Thus, the fiber-shaped battery is well-suited for integration into fabrics. To illustrate its application, two Al–air batteries with fiber-like structures were enclosed in a permeable tube and linked in a series configuration to increase the output voltage and power. Subsequently, these batteries were integrated into a flexible textile to power a light-emitting-diode (LED) watch worn on a human wrist, as shown in Fig. 18(a) and (b).187
Fig. 18 Demonstration pictures of commercial LED watch operated by cabled-Al–air batteries woven into fabric from (a) front and (b) back side.187 (c) Use of aqueous Al–air battery with circulating electrolyte.260 (d) AGE-based flexible wearable Al–air battery showing the potential to charge a mobile phone.243 (e) Ultrathin paper-based battery for powering a fan.237 |
Aqueous electrolyte-based Al–air batteries are appropriate options for stationary purposes given that their ionic conductivity and practical discharge plateau are high. The demonstration using an aqueous rechargeable battery with the LED showing ‘Al–air’ is shown in Fig. 18(c). 3-D printed ultrathin batteries can also be useful for portable purposes, as discussed in Section 7.236–239 The charging of mobile phones and working of a small fan were also demonstrated using polymer-based flexible batteries (see Fig. 18(d) and (e)).237,243 These applications demonstrate the versatility and potential of Al–air battery systems for a wide range of portable and strategic applications, including flexible platforms.
The maintenance of electrolyte stability is crucial for ensuring the optimal functioning of Al–air batteries. However, the process of battery discharging can lead to electrolyte dissolution, evaporation, and side reactions, potentially impacting the performance and safety. Resolving these concerns requires advancements in stable formulations and additives for electrolyte systems. Additionally, understanding the electrolyte degradation mechanisms and developing electrolytes with enhanced stability, conductivity, and compatibility with aluminum anodes are essential research areas. For example, stopping the reaction when required, given that in the non-operating stage it continues to corrode the anode. Al–air batteries depend on uninterrupted oxygen provision from the surrounding atmosphere to maintain their ORR activity. However, controlling the oxygen diffusion and airflow poses significant challenges, particularly in sealed systems. The ingress of CO2 from the atmosphere can deteriorate the battery activity, leading to the formation of insoluble carbonates in alkaline electrolyte, hindering the ionic conductivity and decreasing the power efficiency. Purging of pure oxygen in the battery can mitigate this issue by integrating the suitable design; however, it may increase the battery weight and may require a complicated battery management system. Further, incorporating neutral pH electrolytic media can be beneficial, reducing the likelihood of carbonate formation. Thus, research efforts should be aimed at enhancing the oxygen utilization efficiency and preventing impurities and CO2 dissolution, which is crucial for optimizing the Al–air battery performance. This entails the development of novel air-breathing structures and diffusion layers, and the investigation of sophisticated ventilation methodologies. Achieving optimal efficiency and stability in both anode and cathode materials is essential for the overall Al–air battery performance. Significant challenges persist in developing appropriate catalysts and electrode designs, particularly in the creation of sophisticated air-cathode materials with improved electrochemical characteristics and stability. Research efforts are required to investigate novel catalyst materials, develop nanostructured electrode structures, and understand the kinetics involved in electrode reactions.
To better understand the electrochemical reactions, conventional pre- and post-discharge analysis is performed to understand the reaction mechanism. However, these measurements only provide indirect information, which will not assist in the comprehensive understanding of the changes occurring during the discharge processes. The characteristics of the catalysts are complex and can vary under real electrochemical conditions. In this case, in situ measurements can be helpful. There are some reports in the literature based on lithium– and zinc–air batteries related to in situ operation such as in situ XRD, in situ Raman, and XPS, providing a better understanding of the reaction mechanism and microscopic changes in different charge/discharge states.261,262 Operando XRD can highlight the activity of the metal–air battery by monitoring the ORR process by the detection of the adsorption of oxygen intermediates, resulting in different Al-crystallographic phases.263 Similarly, in situ Raman measurements will also be beneficial with less limitations to check the structural changes and provide details of the interfaces during the discharge/charge process, especially to check the formation of carbonates and any anode surface degradation while interacting with the electrolyte.264 The same strategies of in situ measurements can also be applied to Al–air batteries to overcome the limitations and to control the reaction parameters for both primary (non-rechargeable) and secondary (rechargeable) Al–air batteries.
The goal of sustainability in Al–air batteries necessitates the resolution of obstacles pertaining to the recycling and ecological implications associated with aluminum anodes and electrolyte components. Thus, further investigation is required to establish effective recycling methodologies for the retrieval of aluminum and the regeneration of the electrolyte. Furthermore, it is crucial to evaluate the ecological consequences of Al–air batteries and devise approaches for their sustainable disposal at the end of their lifespan, consequently avoiding new environmental problems, while solving the existing ones.
This journal is © The Royal Society of Chemistry 2024 |